Background

Bulk heterojunction (BHJ) polymer solar cells (PSCs) have been extensively investigated as a new energy substitute due to their low cost, solution processing capability, and flexibility in fabricating large-area devices [16]. So far, the power conversion efficiency (PCE) of BHJ PSCs has recently achieved 9.2% or more [7, 8]. It is very close to the commercialization level. However, there are some factors limiting the efficiency of PSCs, such as low absorption efficiency and narrow absorption range, short exciton diffusion length, low charge carrier mobility, and so on [9, 10]. One of the possible strategies to increase its PCE is to stack two or more cells with different spectra response together as tandem solar cells [8, 11]. It is particularly important to study semitransparent solar cells on the investigation of tandem solar cells. Meanwhile, semitransparent BHJ PSCs are also interesting for other applications, such as power-generating windows [12].

The semitransparent BHJ PSCs require transparent electrodes on both bottom and top sides. There are many researches that focus on top transparent electrodes while the bottom ones typically use indium tin oxide (ITO) electrodes with high transparency in the visible light region [1318]. And these top transparent electrodes may use one type of thin metal (such as the highly reflective anode Al (100 nm) replaced by a transparent layer of Ag (20 nm) or by a transparent layer of Au (12 nm) [13, 14]), may stack two or more thin metals (such as Al/Au (0.5 nm/15 nm) [15, 16]), or may use multilayer composite structure (such as PEDOT:PSS/PH1000/WO x (40 nm/70 nm/20 nm), WO3/Ag/WO3 (10 nm/13 nm/40 nm) [17, 18]) and so on.

In our previous reports [19], ITO substrate semitransparent inverted PSCs were studied. The conductivity of ITO decreased because high-temperature (500°C) annealing must be handled during the preparation of nanocrystalline titanium oxide (nc-TiO2). This report focuses on the fluorine-doped tin oxide (FTO) substrate semitransparent inverted PSCs employing a sol-gel-derived TiO2 electron-selective layer (ESL) and with a multilayer anode structure of MoO3/Ag/MoO3. The inner MoO3 layer, which served as a hole transport material (HTM), is inserted between the active layer and Ag to enhance hole collection, and the outer MoO3 layer is used as a top capping layer to enhance light coupling.

The results show that the replacing FTO substrate enhances light transmittance between 400 and 600 nm but does not change sheet resistance after annealing treatment. Compared to our reported ITO substrate inverted PSCs, high PCE about 75% increase was achieved for the FTO substrate device when illuminated from the FTO side (bottom side) and about 150% increase done when illuminated from the MoO3/Ag/MoO3 side (top side).

Methods

The photovoltaic device has a structure of FTO/nc-TiO2/P3HT:PCBM/MoO3/Ag/MoO3, (P3HT, Luminescence Technology Co., Palo Alto, CA, USA; 95 + % regioregular, electronic grade, PCBM, Luminescence Technology Co., Palo Alto, CA, USA, 99.5 + %) as shown schematically in Figure 1. The FTO conducting glass substrate (with a sheet resistance of <15 Ω/□) was pre-cleaned using acetone, ethanol, and deionized (DI) water for 15 min each. Anatase phase TiO2 thin films were prepared through a sol-gel method similar to our previous papers [20, 21]. The procedure for the preparation of TiO2-sol involved the dissolution of 10 ml Ti(OC4H9)4 in 60 ml ethanol (C2H5OH), followed by adding 10 ml acetyl acetone. Then, a solution, composed of 30 ml C2H5OH, 2 ml DI water, and 2 ml hydrochloric acid (HCl) with a density of 0.28 mol/l, was added dropwise under vigorous stirring. The final mixture was stirred at room temperature for 24 h. Subsequently, TiO2-sol was spin cast on FTO conducting glass substrates at 3,000 rpm for 40 s. Then, the samples were annealed at 500°C for 30 min in a muffle furnace. The typical thickness of TiO2 is 25 nm. For the active layer, P3HT (used as received) was dissolved in 1,2-dichlorobenzene to produce an 18-mg/ml solution, followed by blending with PCBM (used as received) in 1:1 weight ratio [22]. The blend was stirred for 24 h in a nitrogen-filled glovebox before spin coating on top of the TiO2 film surface. Then, the samples were annealed at 150°C for 10 min on a hot plate in the glovebox. The typical film thickness of P3HT:PCBM was about 100 nm. Finally, 1 nm of MoO3, 10 nm of Ag, and x nm (x =20, 40, 60, and 80 nm) of MoO3 were thermally evaporated in sequence under high vacuum (5 × 10-4 Pa) without disrupting the vacuum. The deposition rate which was monitored with a quartz-oscillating thickness monitor (CRTM-9000, ULVAC, Methuen, MA, USA) was about 0.05 nm/s. The active area of the device was about 4 mm2.

Figure 1
figure 1

Schematic structure drawing of semitransparent inverted polymer solar cells.

Current density-voltage (J-V) characteristics were measured using a computer-programmed Keithley 2400 source meter (Keithley 2400, Keithley Instruments, Inc., Cleveland, OH, USA) under AM1.5G solar illumination using a Newport 94043A solar simulator (Newport 94043A, Oriel, Irvine, CA, USA). The intensity of the solar simulator was 100 mW/cm2. Light intensity was corrected by a standard silicon solar cell. The transmission and reflection spectra were measured using ultraviolet/visible (UV-VIS) spectrometer (Carry 5000, Agilent Technologies, Inc., Santa Clara, CA, USA). The resistivity and sheet resistance were measured using four-point probe resistivity measurement (JG SZT-C).

Results and discussion

As shown in Figure 2a, the J-V characteristic curves of the device FTO/nc-TiO2/P3HT:PCBM/MoO3 (1 nm)/Ag (10 nm)/MoO3 (x nm) (x =20, 40, 60, and 80 nm) under AM1.5G solar illumination of 100 mW/cm2 in ambient air when illuminated from the FTO side (bottom). The detailed results are given in Table 1. Compared with our previous results [19] (the device has a structure of ITO/nc-TiO2/P3HT:PCBM/MoO3 (1 nm)/Ag (10 nm)/MoO3 (x nm)), there is a similar variation that the PCE increases with increasing MoO3 thickness when illuminated from the FTO electrode. It is known that reflectance of the top electrode plays an important role in trapping light for the active layer to reabsorb. The reflectance peaks of the MoO3/Ag/MoO3 electrode are redshifted and would match better to the absorption spectra of the active layer (400 to 650 nm) when the thickness of the MoO3 capping layer increases [19, 20]. As a result, high PCE is achieved for FTO substrate inverted PSCs, which shows about 75% increases compared to the reported ITO substrate device at different thicknesses of the MoO3 capping layer of the MoO3/Ag/MoO3 transparent electrode films. The PCE increases from 1.40% to 2.43%, 1.55% to 2.62%, 1.64% to 2.87%, and 1.76% to 3.09% at MoO3 capping layer thicknesses of 20, 40, 60, and 80 nm, respectively.

Figure 2
figure 2

J - V characteristics. J-V characteristics of device FTO/nc-TiO2/P3HT:PCBM/MoO3 (1 nm)/Ag (10 nm)/MoO3 (x nm) (x =20, 40, 60, and 80 nm) depending on the thickness of the MoO3 capping layer when illuminated from (a) the ITO side and (b) the MoO3/Ag/WO3 side.

Table 1 Characteristic data of semitransparent inverted polymer solar cells

When illuminated from the MoO3/Ag/MoO3 electrode side (top), the efficiency decreases from 2.19% to 1.62% with increasing thickness of MoO3. This phenomenon, which is similar with that of the reported ITO substrate devices (0.96% to 0.60%), might result from the reduced transmittance of MoO3/Ag/MoO3 between 400 and 650 nm when increasing the MoO3 thickness. Figure 2b shows the J-V characteristic curves. The detailed results are given in Table 1. Meanwhile, PCE for FTO substrate inverted PSCs shows about 150% increase compared to the reported ITO substrate. The PCE increases from 0.96% to 2.19%, 0.82% to 1.99%, 0.72% to 1.84%, and 0.60% to 1.64% at MoO3 capping layer thicknesses of 20, 40, 60, and 80 nm, respectively.

One reason of these increases might be that the impact of FTO substrate samples on the environment is reduced, in which the process was in a nitrogen-filled glovebox while the reported process was in the air. The second reason might be that the resistivity of the ITO substrate increases after annealing treatment at high temperature while the resistivity of the FTO substrate does not. For ITO, the oxygen hole as carrier reduction causes the decrease of conductivity after annealing. The third reason might be that the light transmittance of the FTO substrate was a little higher than that of the ITO substrate.

Here, we measured the resistivity of ITO and FTO substrates after annealing treatment at different temperatures (T =20°C, 100°C, 200°C, 300°C, 400°C, and 500°C) for 30 min. The curve is shown in Figure 3. For the ITO substrate, resistivity has a little change while annealing temperature is below 200°C and increases while annealing temperature is more than 300°C obviously. For the FTO substrate, resistivity has little change while annealing temperature is below 500°C. The inset in Figure 3 is the corresponding square resistance. For the ITO substrate, square resistance is 7.96 Ω/□ when annealing temperature is at 20°C and 40.65 Ω/□ at 500°C. It is about five times over. For the FTO substrate, square resistance is 13.48 Ω/□ when annealing temperature is at 20°C and 13.61 Ω/□ at 500°C which are of almost equal values. Because the oxygen holes as conductive carriers in the ITO decrease after 300°C annealing, the resistivity and sheet resistance increase. For FTO, this temperature is above 500°C. This is well matched with the causes.Figure 4 shows the transmittance spectra of ITO and FTO substrates after annealing treatment at 20°C and 500°C for 30 min and the absorption spectra of the P3HT:PCBM active layer. The absorption spectra range of the active layer is approximately 400 to 650 nm. In this range of wavelength, it can be seen that the transmittance of the FTO substrate is over 85% which is higher than that of the ITO substrate (between 75% and 85%). The active layer of the FTO substrate device can receive more sunlight than that of the ITO substrate device in a wavelength range of 400 to 650 nm. Meanwhile, the transmittance has been roughly unchanged after annealing at 500°C for the FTO substrate. For the ITO substrate, the transmittance has reduced and has a slight redshift. It might be caused by the reduction of oxygen vacancies.

Figure 3
figure 3

Resistivity of ITO and FTO substrates after annealing treatment at different temperatures. T =20°C, 100°C, 200°C, 300°C, 400°C, and 500°C for 30 min. The inset shows the corresponding square resistance.

Figure 4
figure 4

Transmittance spectra of ITO and FTO substrates after annealing treatment at 20°C and 500°C. The hollow star line is the absorption spectra of P3HT:PCBM active layer.

Conclusions

In summary, we demonstrated conductive FTO substrate semitransparent inverted PSCs with high-temperature annealing of nc-TiO2 as an electron-selective layer. The performances of PSCs with different substrates and different thicknesses of the MoO3 capping layer are investigated and compared. As a result, higher PCE was achieved for FTO substrate semitransparent inverted PSCs than that for the ITO substrate both illuminated from the bottom side and from the top side. For structurally identical PSCs, with increasing thickness of the MoO3 capping layer, the PCE is enhanced when illuminated from the bottom side but decreased when illuminated from the top side.