Location via proxy:   [ UP ]  
[Report a bug]   [Manage cookies]                

Tabela Materiais PDF

Fazer download em pdf ou txt
Fazer download em pdf ou txt
Você está na página 1de 1

Materials / technical parameters

Ductile iron – according to DIN EN 1563 – selection


Guaranteed properties on separately cast test specimens*
Letter Material Diameter Tensile 0,2 -%- Elongation at Brinell Essential
symbol number of the tensile strength Yield rupture hardness structural
test specimen Rm strength % HB constituents
mm N/mm² N/mm²
ferritic/
EN-GJS-400-15 5.3106 12 400 250 15 135-180 pearlitic
ferritic/
EN-GJS-500-7 5.3200 12 500 320 7 170 –230 pearlitic
ferritic/
EN-GJS-600-3 5.3201 12 600 380 3 200 –250 pearlitic
predominantly
EN-GJS-700-2 5.3300 12 700 420 2 235 –285 pearlitic
EN-GJS-400-18-
LT 5.3103 12 400 240 18 130 –165 ferritic
EN-GJS-450-18 5.3108 12 450 350 18 170-200 ferritic
EN-GJS-500-14 5.3109 12 500 400 14 185-215 ferritic
EN-GJS-600-10 5.3110 12 600 470 10 200-230 ferritic
With silicon and molybdenum alloyed cast iron with nodular graphite according to DIN EN 16124 Selection – excerpt
EN-GJS- predominantly
SiMo45-10 5.3117 12 550 460 5 200-250 ferritic
* Particularly in case of wall thicknesses of more than 50 mm and compact cast parts, we recommend agreements between the
manufacturer and the consumer.

Ausferritic ductile iron (ADI) – according to DIN EN 1564


Letter Material Diameter Tensile 0,2 -%- Elongation at Brinell Essential
symbol number of the tensile strength Yield rupture hardness structural
test specimen Rm strength % HB constituents
mm N/mm² N/mm²
austenitic/
EN-GJS-800-10 5.3400 12 800 500 10 250-310 ferritic
austenitic/
EN-GJS-900-8 5.3402 12 900 600 8 280-340 ferritic
austenitic/
EN-GJS-1050-6 5.3403 12 1050 700 6 320-380 ferritic
austenitic/
EN-GJS-1200-3 5.3404 12 1200 850 3 340-420 ferritic
austenitic/
EN-GJS-1400-1 5.3405 12 1400 1100 1 380-480 ferritic

Gray cast iron – according to DIN EN 1561 – selection


Guaranteed properties on separately cast test specimens *
Letter Material Diameter Tensile Brinell Essential
symbol number of the tensile strength hardness structural
test specimen Rm HB constituents
mm N/mm²
EN-GJL-150 5.1200 20 150 –250 165 –205 ferritic/pearlitic
EN-GJL-200 5.1300 20 200 –300 185 –225 pearlitic
EN-GJL-250 5.1301 20 250 –350 205 –250 pearlitic
EN-GJL-300 5.1302 20 300 –400 225 –270 pearlitic
* Tensile strength and Brinell hardness in the cast part strongly depend on the wall thickness.

Malleable cast iron – according to DIN EN 1562 – selection


Letter Material Diameter Tensile 0,2 -%- Elongation at Brinell Essential
symbol number of the tensile strength Yield rupture hardness structural
test specimen N/mm² strength % max. HB constituents
mm N/mm2
EN-GJMW-400- 9 360 200 8 220 core: (lamellar to fine-grained )
5 EN-JM 1030 12 400 220 5 220 perlite + temper carbon
EN-GJMW-450- 9 400 230 10 220 Core: (grained)
7 EN-JM 1040 12 450 260 7 220 perlite + temper carbon
Decarburization to
EN-GJMW-360- 9 320 170 15 220 < 0,3 % C-content in case of
12 EN-JM 1020 12 360 190 12 220 wall thicknesses of < 8 mm
Alloyed types of material upon request.