Location via proxy:   [ UP ]  
[Report a bug]   [Manage cookies]                
Next Article in Journal
Petal-like g-C3N4 Enhances the Photocatalyst Removal of Hexavalent Chromium
Previous Article in Journal
A Review of Transition Metal Nitride-Based Catalysts for Electrochemical Nitrogen Reduction to Ammonia
Previous Article in Special Issue
Stable Nickel-Based Metal–Organic Framework Containing Thiophene/Diimidazole Units for Effective Near-Infrared Photothermal Conversion
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Ethylene Dimerization Performance of NiBTCs Synthesized Using Different Solvents

State Key Laboratory of Fine Chemicals, School of Chemical Engineering, Dalian University of Technology, Dalian 116024, China
*
Author to whom correspondence should be addressed.
Catalysts 2023, 13(3), 640; https://doi.org/10.3390/catal13030640
Submission received: 13 February 2023 / Revised: 16 March 2023 / Accepted: 20 March 2023 / Published: 22 March 2023
(This article belongs to the Special Issue MOFs Catalyst for Energy-Related Reactions)

Abstract

:
MOFs have attracted widespread attention in the field of catalytic ethylene dimerization. Compared with post-synthetic modification, ion exchange and other methods to introduce external active centers, the direct use of MOF materials as catalysts is still the most convenient and prospective. Herein, the NiBTCs are synthesized using a one-pot method in two kinds of solvent and characterized by XRD, FT–IR, ICP–OES, XPS, TGA and N2 physical adsorption. After treatment at 150 °C, the catalytic activities of both materials in ethylene dimerization are up to 470.9, and 647.0 gpro./(gcath) and the selectivity of 1-butene in all products could reach 83.2% and 81.7%, respectively. Stability testing of the catalysts demonstrated that they do not decompose during the reaction, but their reuse performance is degraded. In addition, a probable Cossee–Arlman–type mechanism is proposed. The NiBTCs are shown to have superior catalytic performance in ethylene dimerization compared to employing Ni(pyz)2Cl2 or α–Ni(im)2 as catalysts.

Graphical Abstract

1. Introduction

To benefit from increasing ethylene production, ethylene dimerization has been the focus of researchers’ attention since synthesising important industrial feedstocks such as sec-butanol, butadiene and isoprene require large amounts of 1-butene [1,2,3]. Compared with other metal catalysts, the most widespread process for ethylene dimerization relies on Ni, attributed to its low cost and unique reactivity with unsaturated organics [4,5,6]. For instance, Chen et al., used NiCl2{(6E,13E)-N1,N4-bis(1-(pyridin-2-yl)ethylidene)benzene-1,4-diamine}NiCl2 as the catalyst in the presence of diethylaluminum chloride (Et2AlCl), the activity was up to 869.1 gpro./(gcath) at 20 bar, 50 °C [7]; Feng et al., utilized syn-Ni2(C52H38Br4N2Ni2P2)/EtAlCl2, the activity of reaction could reach 15,307 gpro./(gcath) [8]. The above homogeneous studies demonstrated the high reactivity of nickel as the active center, but the homogeneous catalytic system still suffers from a complex synthesis process and difficult catalyst recovery, which limits further developments. Heterogeneous catalytic systems can effectively solve the above problems, but improving the reactivity and product selectivity, especially for 1-butene, is still an important challenge to be faced [9].
Metal–organic frameworks (MOFs) are solid-phase porous materials composed of organic ligands and metal clusters [10,11,12,13,14]. Similar to homogeneous catalysts, they possess rich coordination patterns and diverse organic ligand structures, which provide a feasible idea for efficient catalytic ethylene dimerization in heterogeneous phases [15]. The studies of Ni-MOFs catalysts showed that the coordination of unsaturated sites (CUS) in the materials could effectively improve the catalytic activity in ethylene dimerization [16,17,18]. CUS-containing MOFs are currently prepared in the following ways: (1) Post-synthetic modification to introduce a new active center, e.g., Canivet et al., grafted Ni(2–PyCHO)Cl2 in NH2–MIL(Fe)–101 to form Ni@(Fe)MIL–101 for ethylene dimerization with a maximum activity of 205.0 gpro./(gcath) [19]. (2) Creation of active centers by ion exchange, e.g., Metzger et al., replaced a portion of Zn in MFU-4l with Ni by ion exchange, resulting in the formation of CUS. The activity was up to 198.0 gpro./(gcath) at 50 bar, 25 °C, and the selectivity of 1-butene in the product reached 92.0% [20]. (3) Creation of active centers by inconsistent coordination mode, e.g., Chen et al., used a one-pot method to add a certain amount of Ni to the synthesis of ZIF-8 to form the CUS. The reactivity reached 2130 gpro./(gcath) at 35 °C, 30 bar, and the selectivity of 1-butene in the product reached 85.1% [21]. (4) Removal of solvent molecules ligated to the active center in the structure of the MOF, e.g., Hu et al., reported that Ni-UMOFNs require activation at 190 °C in a vacuum oven to achieve better catalytic activity and 1-butene selectivity (5536 h−1 and 75.6%) [17]. Comparing these methods indicates that the fourth way is the most convenient and has relatively better prospects for industrial applications, which is worth exploring further.
NiBTC was firstly synthesized from nickel(II) acetate tetrahydrate and 1,3,5-benzene tricarboxylic acid (H3BTC) through a classical hydrothermal reaction, which is reported by O. M. Yaghi and coworkers [22]. Subsequently, NiBTCs with different coordination modes have been synthesized by changing the synthesis conditions (e.g., reaction temperature, reaction time, solvent type and additives required for crystallization), which have been widely used, such as OER, supercapacitor, anode material for Li-ion batteries and catalysts for the reaction of CO2 cycloaddition [23,24,25]. In general, a benzene tricarboxylic acid ion is coordinated to four nickel atoms with two multidentate carboxylate groups in the structure of NiBTCs. In order to complete the octahedral environment of the nickel center, the remaining two empty coordination sites are occupied by water molecules (or solvent molecules) (Figure 1), which can be dispelled to form CUS active centers [26]. This is the key to how NiBTC can be used in the aforementioned research, so the reactivity of NiBTC materials in ethylene dimerization is expected.
In this work, we synthesized two NiBTCs using a one-pot method in different solvents and applied them as catalysts in the dimerization of ethylene. The activities of the NiBTCs were up to 470.9, and 647.0 gpro./(gcath), and the selectivity of 1-butene in all products could reach 83.2% and 81.7%, respectively. The fresh and used catalysts were also characterized by inductively coupled plasma optical emission spectrometer (ICP–OES), X-ray diffraction (XRD), Fourier transform infrared spectroscopy (FT–IR), X-ray photoelectron spectroscopy (XPS), thermogravimetric analysis (TGA) and N2 physical adsorption. Two other MOFs (Ni(pyz)2Cl2 and α–Ni(im)2) were also synthesized to compare the catalytic activity with the NiBTCs. Moreover, a possible ethylene dimerization mechanism of NiBTC was proposed with the inspiration of the Cossee–Arlman mechanism.

2. Results and Discussion

2.1. Characterization

The synthesis process of the two NiBTCs is described in Section 3.2. XRD patterns are used to investigate the structure of the NiBTCs. As shown in Figure 2A, the NiBTC–DMF presents two distinct diffraction peaks at 11° and 23° corresponding to the (100) and (101) planes, respectively, which broaden in NiBTC–EtOH. The phenomenon observed in this work is similar to the results previously reported in NiBTC synthesis [23,24]. The FT–IR spectra clearly show peaks for the NiBTC–DMF and NiBTC–EtOH in Figure 2B. The wide peak centered at 3408 cm−1 is attributed to the stretching mode of hydroxyl (O–H) groups from absorbed water, and the bands in the region of 780–722 cm−1 correspond to the in-plane as well as the out-of-plane deformation vibrations of the C-H groups in the benzene ring [28]. Meanwhile, by magnifying the part of 1800–1200 cm−1 (Figure 2C), it can be seen that the adsorption bands of -COOH, which relate to the BTC ligands and formic ligands, are not observed in the expected region at 1800–1680 cm−1 [22,29]. On the other hand, the characteristic bands of coordinated -COO groups located at 1618–1559 cm−1 (asymmetric vibration) and 1436–1307 cm−1 (symmetric vibration) are detected in the corresponding spectral region [30,31]. All of the above implies that the BTC and formic ligands have coordinated with the metal ions [32]. It is also noteworthy that two distinct absorption peaks are present in the structure of NiBTC–DMF alone; the peaks at 2168 cm−1 and 1113 cm−1 should be attributed to the tertiary amine group and the stretching vibration of C-N, respectively [24,33]. These two absorption peaks also prove the presence of the solvent DMF molecule in the structure of NiBTC–DMF.
XPS characterization was carried out, and the corresponding results are presented in Figure 3. The survey spectra of the NiBTCs (Figure 3A) exhibit three obvious peaks at 285 (C 1 s), 531 (O 1 s) and 856 (Ni 2p3), suggesting the formation of MOFs. For the Ni 2p core level XPS spectra, as shown in Figure 3B, two major peaks positioned at 855.6 and 873.1 eV can be assigned to the splitting of Ni 2p 3/2 and Ni 2p 1/2, a spin–energy separation of 17.5 eV could be calculated from the major peaks, also confirming the presence of Ni2+ [34,35,36]. The deconvoluted higher binding energy peaks at 857.0 and 874.5 eV may be attributed to the trace amount of Ni3+, which may be generated by the hydrothermal and oxidative effects during the crystallization process [37,38]. The broad peaks located at 861.7 eV and 879.7 eV are the satellite peaks of Ni 2p 3/2 and Ni 2p 1/2. Furthermore, Figure 3C shows the spectra of C 1 s, with the three main peaks at 284.8 eV (C–C), 285.6 eV (C–O) and 288.2 eV (C=O) nearby, which is in good agreement with the bonding mode of element C in NiBTC. Figure 3D displays the spectra of O 1 s, and the O peak at 531.2 eV is typical of Ni–oxygen (Ni-O) bonding and the deconvoluted binding energy peaks at 533.0 eV may be attributed to C-O bonding [39].
Thermogravimetric analyses at 40–600 °C are performed under an N2 atmosphere, and the results are shown in Figure 4A,B. Each thermogram of the NiBTCs has three distinct regions at different temperature ranges. Their initial weight loss steps (NiBTC–DMF, 40–178 °C and NiBTC–EtOH, 40–229 °C) are attributed to the loss of water molecules and some of the solvent molecules in coordination [40,41]. As the heating continued, their structures became unstable. The weight losses of 16.7 and 17.3% in the same sequence are attributed to the further separation of solvent molecules (DMF, EtOH) from the structure until 350 and 361 °C, respectively [24,42]. The network of NiBTCs collapses completely when the temperature is higher than 450 °C [43]. The results above further prove that the water molecules exist in the NiBTCs, which is in accordance with the FT–IR, and also demonstrate that two NiBTCs can get rid of H2O and some solvent molecules by heat treatment below 178 and 229 °C, respectively, to form CUS.
The NiBTCs present a typical type–IV isotherm with an H4–type hysteresis loop starting from P/P0 ≈ 0.45, indicating the presence of interparticle buildup (Figure 4C). The specific surface area of NiBTC–DMF (60.91 m2/g) is somewhat higher than the values reported previously (40.36 m2/g) [24]. This is primarily because the material was subjected to the activation process following synthesis, which is commonly performed to achieve a high surface area for the MOFs [27]. In addition, the micropore area and volume of the NiBTCs are calculated to be approximately equal to 0 by the t-plot method, which is consistent with the same type of NiBTCs [24,44,45,46]. This proves that they may not possess the microporous structure possessed by MOFs in general, and thus their specific surface area is lower than that of other structural NiBTCs [42,47].

2.2. Ethylene Dimerization

The catalytic performance of NiBTC–DMF is shown in Figure 4. The effect of the Al/Ni molar ratio on the catalytic performance of NiBTC–DMF in ethylene dimerization is investigated in Figure 5A. With the increase of the Al/Ni molar ratio from 50 to 200, the catalytic activity first increases and then decreases. The product distribution gradually shifts toward the high carbon number with an increase of Et2AlCl. However, the obtained ≥C8 products are not linear α-olefins but branched olefins as well as other impurities, so it can be basically speculated that the addition of excess Et2AlCl may interfere with the formation of active species and lead to the over-reduction of the active center, which is consistent with the reports in the literature [48]. The effects of different temperatures on the catalytic activity of NiBTC–DMF are shown in Figure 5B. The reactivity rises gradually with the increase of temperature from 20 to 50 °C, reaching a maximum of 196.9 gpro./(gcath) at 50 °C. After that, the reactivity shows a large decrease with the increase in temperature. The dimerization is exothermic, and increasing the temperature will further lead to a decrease in the solubility of ethylene in the solvent, thus leading to a decrease in activity [49]. The activity decreases from 196.9 gpro./(gcath) to 153.0 gpro./(gcath) when the amount of catalyst is reduced from 0.005 g to 0.003 g (Figure 5C), indicating that the number of active centers of the catalyst also affects the dimerization reaction. Therefore, it concluded that the best performance of the catalyst could be obtained at 0.005 g, Al/Ni molar ratio of 100 and a temperature of 50 °C based on the above.
Under these optimal conditions, we compare the activity of the NiBTC–DMF and NiBTC–EtOH as shown in Table 1. There is no product only in the presence of Ni(NO3)2·6H2O, H3BTC and Et2AlCl or only in the presence of H3BTC and Et2AlCl, which indicates that it is the MOFs instead of metal source or organic ligands that possess the catalytic activity in the reaction. The activity of NiBTC–EtOH is always higher than NiBTC–DMF’s, but the selectivity of 1-butene has the opposite trend. The reason may be that the active center in NiBTC–EtOH with low crystallinity is more fully exposed, so its activity is higher, but the effect of the surrounding ligands on the β-H elimination is relatively weakened at the same time. As a result, 1-butene stays in the active center, and further branching reactions occur. After extending the reaction time, we find that the activity of both catalysts decreases, indicating that many products may block or cover the active center. Thus, NiBTC–EtOH, with more active centers, exhibits higher reactivity (279.4 > 157.2 gpro./gcathࢤ1) in the reaction. The TOF value of the catalysts is calculated based on the Ni content in Section 3.2.

2.3. The Stability of Catalyst

To verify the stability of the catalyst in solution, we separate the filtrate of the reaction under anhydrous and oxygen-free conditions and put the filtrate back into the reaction. The result of the leaching test shows that the reaction does not proceed any further, even in the presence of an Al-based co-catalyst (Table 2), which demonstrates that the catalytic system is always a heterogeneous system.
The recovered catalysts are fully washed with anhydrous ethanol, dried and further tested after being reactivated. The results are shown in Table 3. The activity of both materials decreases, with NiBTC–DMF decreasing to 54% of the original activity and NiBTC–EtOH decreasing to 41%. In order to determine the factors involved, the catalysts are characterized by ICP–OES, XRD and FT–IR after the first reaction. It can be seen that the percentage of Al in the spent catalyst increases significantly, indicating that some of the Et2AlCl hydrolysis products are attached to the catalyst [21]. The XRD patterns of the recovered catalysts show a significant decrease in the crystallinity, while the shape of the original peaks remains essentially unchanged in Figure 2A. Visibly, new diffraction peaks appear at 21.5°, indicating a change in the crystal structure of both materials. FT–IR spectra show a decrease in the intensity but no change in the position of the absorption peaks for both materials in Figure 2B and C. Additional absorption peaks appear at 2918 cm−1 and 2850 cm−1, which are attributed to the stretching vibration peaks of alkanes. All of the above indicates that Al-impurities cover the active center, and some alkyl groups are embedded in the skeletons of both materials, resulting in decreased activity of the recovered catalysts.

2.4. Postulated Mechanism for Ethylene Dimerization

According to the above results, we propose a possible mechanism for the NiBTCs-catalyzed ethylene dimerization, as shown in Figure 6A. At first, NiBTC is activated by the high temperature at 150 °C to eliminate the water/solvent molecules in the structure, followed by further activation by Et2AlCl to form Ni-H active centers. Then, an incoming ethylene is coordinated to the active Ni, followed by the ethylene insertion and producing intermediates Ni-C2H5. After another ethylene subsequently coordinates to Ni-C2H5 and inserts into the C-H bond, the Ni-C4H9 is formed. The β-H elimination of Ni-C4H9 would generate 1-butene as well as release the active center. When the β-H elimination does not occur in time, further branching reactions are carried out [20]. The generation of the C6 products is essentially the same as that of the C4 products through an insertion–elimination process. The distribution of the resulting C4 products (1-butene, cis-2-butene, trans-2-butene and isobutene) and C6 products (3-methyl-1-propene, 1-hexene, 2-ethyl-1-butene, 3-hexene, 2-hexene and benzene) (Figure 6B) are similar to previous studies [50]. Combining with other reported reaction mechanisms of nickel-based catalysts, we suggest that NiBTCs follow the Cossess–Arlman type mechanism for the reaction [51,52,53].

2.5. Comparison with Other Catalysts

In this work, the Ni(pyz)2Cl2 and α–Ni(im)2 are characterized by XRD and FT–IR (Figure 7A,B). It can be seen that the simulated and experimental XRD patterns are in good agreement with each other, which proves the phase purity of the as-synthesized samples [54,55]. In FT–IR spectra, the weak peaks in the range of 3143–3108 cm−1 are attributed to the stretching mode of C-H on the heterocyclic compounds and the range of 825–665 cm−1 is attributed to the out-of-plane bending vibration of C=N [56]. By magnifying the part of 1800–1200 cm−1 (Figure 7C), for Ni(pyz)2Cl2, the band at 1636 cm−1 and the range of 1487–1417 cm−1 are attributed to the stretching vibrations C=C and C-H groups, respectively. The band at 1390 cm−1 is assigned to the stretching vibration of C=N [57]. Unlike Ni(pyz)2Cl2, it can be stated that the stretching vibrations of C=N are superimposed at 1587 cm−1 for α–Ni(im)2 [58]. The stretching vibrations of C=C and C-N groups are located in the range of 1689–1619 cm−1 and 1489–1470 cm−1, respectively [59]. In addition, the peaks at 1321–1233 cm−1 correspond to the in-plane bending of the imidazole rings [60].
The catalysts are subjected to ethylene dimerization under the same reaction conditions (Table 4), and the results show that the activity and TOF values of the two NiBTCs are higher than those of the other two materials. The reason may be that the coordination site of Ni(pyz)2Cl2 was occupied by Cl, which needed to be replaced by an active group in the aluminum co-catalyst for further reaction, while α–Ni(im)2 is a four-ligand structure with a large space resistance around the empty coordination site, so their activity is relatively lower.
The activities of NiBTCs in ethylene dimerization are also compared with other reported catalysts in Table 5, which indicates that better activity and selectivity of 1-C4 can be achieved using NiBTCs under optimal reaction conditions.

3. Materials and Methods

3.1. Reagents and Instruments

Ni(NO3)2·6H2O (98%), Ni(CH3COO)2·4H2O (98%), NiCl2·6H2O (98%), n-heptane (98.5%) and ethanol (99.7%) were purchased from Tianjin Damao Chemical Reagent Factory (Tianjin, China). Imidazole (99%), pyrazine (99%) and Et2AlCl (1.0 M solution in toluene) were purchased from Aladdin Biochemical Technology Co., Ltd. (Shanghai, China). H3BTC (99%) was purchased from J & KCHEMICAL Ltd. (Beijing, China). Toluene (99.8%) and acetone (99.9%) were purchased from Tianjin Kemiou Chemical Reagent Co., Ltd. (Tiangjin, China). N, N-dimethylformamide (DMF; 99%) was purchased from Tianjin Fuyu Fine Chemical Co., Ltd. (Tianjin, China). Deionized water was used in all the experimental processes.
XRD patterns are performed at a scanning speed of 0.15 s/step on a Bruker D8 Advance diffractometer (Bruker, Karlsruhe, Germany) equipped with Cu Kα radiation (λ: 1.5418 Å; voltage: 40 kV; current: 40 mA) in the range of 5–80° with a step of 0.025°.
FT–IR spectra are obtained using a Bruker EQUINOX55 spectrometer (Bruker, Karlsruhe, Germany) from 400 cm−1 to 4000 cm−1 by the standard KBr disk method.
ICP–OES analysis is obtained using a PerkinElmer Avio 500 plasma emission spectrometer (PerkinElmer, Waltham, MA, USA).
XPS analysis is obtained using a Thermo Scientific K–Alpha+ spectrometer (ThermoFisher, Waltham, MA, USA) with Al Ka radiation (1486.6 eV). The binding energy (B.E.) spectrum was calibrated according to the C 1s standard spectrum (B.E. = 284.8 eV). The composition on the surface of the catalysts according to the atomic ratios was calculated, and the Linear background and Gaussian–Lorentzian methods were used for peak analysis.
TGA curves were obtained by a TGA8000–Frontier–Clarus SQ8T (PerkinElmer, Waltham, MA, USA) from 30 to 600 °C at a ramping rate of 10 °C/min in N2.
The specific surface area of the synthesized NiBTCs was calculated using the Brunauer–Emmett–Teller (BET) equation based on the N2 adsorption–desorption isotherms (collected at 77 K) recorded by a Micromeritics AutoChem II 2920 instrument (Micromeritics, Norcross, GA, USA).

3.2. Catalysts Preparation

NiBTC–DMF and NiBTC–EtOH. The procedure to synthesize NiBTC–DMF was similar to previously reported literature with a few modifications [24]. 3.0 mmol of Ni (NO3)2·6H2O (0.8724 g) and 0.5 mmol of H3BTC (0.1050 g) dissolved in 60 mL DMF. Thereafter, the mixed solution was stirred for 1 h at room temperature, then transferred into a 100 mL Teflon-lined autoclave at 150 °C for 12 h. After cooling to room temperature, the precipitate was centrifuged and washed with DMF and ethanol several times. Finally, the obtained product was dried in the oven for 24 h at 80 °C. The synthesis process of NiBTC–EtOH was basically the same as the NiBTC–DMF, except that 60 mL DMF was replaced by 60 mL EtOH. A schematic illustration of the synthesis procedure and the probable structure for the NiBTCs is shown in Scheme 1.
Ni(pyz)2Cl2. The procedure to synthesize Ni(pyz)2Cl2 was similar to previously reported literature with a few modifications [54]. A weight of 0.4 g (5.0 mmol) pyrazine was dissolved in 15 mL of acetone and added slowly dropwise with stirring to 10 mL of a water solution containing 0.594 g (2.5 mmol) of NiCl2∙6H2O. After stirring for 1 h, a greenish-white precipitate was obtained by centrifugation, repeatedly washed with water and acetone, and dried under a vacuum. A schematic illustration of the synthesis procedure and the structure for Ni(pyz)2Cl2 is shown in Scheme 2.
α–Ni(im)2. The procedure to synthesize α–Ni(im)2 was similar to the previously reported literature with a few modifications [55]. Imidazole (1.17 g, 17 mmol) was added to 50 mL of aqueous nickel (II) acetate (500 mg, 2.83 mmol) to obtain a dark blue solution. After adding ammonia solution (5 mL) drop by drop, the solution was allowed to stand for about 30 min, heated to 100 °C and stirring was started. After 5 h of reaction, a yellow precipitate was obtained, filtered, washed with deionized water (4 × 30 mL) and acetone (2 × 30 mL), and dried under vacuum at 80 °C for 12 h. A schematic illustration of the synthesis procedure and the structure for α–Ni(im)2 is shown in Scheme 3.
The yields of all catalysts above and the Ni content are shown in Table 6.

3.3. Catalytic Test

Ethylene dimerization was performed in a 200 mL stainless steel autoclave with mechanical stirring, in which 5 bar N2 (three times) and 10 bar ethylene (once) were used to replace air. Then, the autoclave was filled with 70 mL of catalyst solution, including aluminum additive (1 M Et2AlCl in toluene), powdered catalyst, and toluene (solvent). After 30 min, the reaction was stopped by placing it in an ice water bath, and the gas mixture was collected with gas bags. Then, 1 mL of the liquid phase (cooled by ice water and separated from the catalyst by centrifugation) was taken as the sample to be measured by the internal standard method (20 μL n-Heptane is the internal standard). All catalytic data were repeated at least twice, and the error limit of TOF is about ± 4%.
In all cases, the gaseous products were quantified by GC (Techcomp 7890F) equipped with a TM–Al2O3/S column (50 m × 0.53 mm × 25 μm) at 80 °C, direct ramp up to 180 °C. Liquid phase products were quantified by GC (Agilent 6890, Santa Clara, CA, USA) equipped with an HP–5 column (30 m × 0.32 mm × 0.25 μm) at 35 °C for 5 min, heated at 10 °C/min until the temperature achieved 280 °C, which should be maintained 40 min. All of them were coupled with a flame ionization detector (FID).
The activity of the catalyst, the TOF value and the selectivity of the product are calculated from the following equations:
Activity   g p r o . / g c a t . · h = m a l l   p r o d u c t s   g × m cat . g 1 × t   h 1
TOF   =   m C 2 H 4 C o n v . g ×   M C 2 H 4 1 × n Ni mol 1 × t   h 1
m C 2 H 4 C o n v . g = m a l l   p r o d u c t s   g  
where in the mass of converted C2H4   ( m C 2 H 4 C o n v . ) is equal to the mass of all oligomer products m a l l   p r o d u c t s
Selectivity %   = m x g × m a l l   p r o d u c t s   g 1 × 100 %
mx (x = 1-C4, Other C4, C6 and ≥C8)

4. Conclusions

Two materials, NiBTC–DMF and NiBTC–EtOH, were synthesized by the one-pot method in two kinds of solvent and characterized by XRD, FT-IR, ICP-OES, XPS, TGA and N2 physical adsorption. After treatment at 150 °C, the catalytic activity of the two materials in ethylene dimerization could reach 470.9 and 647.0 gpro./(gcath), and the selectivity of 1-butene in all products could reach 83.2% and 81.7%, respectively, under optimal conditions. Stability testing demonstrated that the catalysts do not decompose during the reaction, but the reusability of catalysts decreases significantly. Furthermore, a probable Cossee–Arlman–type mechanism is proposed. This study reveals the unique potential of CUS-containing MOFs materials in ethylene dimerization.

Author Contributions

Data curation, C.W.; investigation, C.W.; methodology, C.W.; supervision, G.L.; validation, C.W. and G.L.; project administration G.L. and H.G.; writing-original draft, C.W.; writing-review and editing, G.L. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Data Availability Statement

Data are contained within the article.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Chen, C. Designing catalysts for olefin polymerization and copolymerization: Beyond electronic and steric tuning. Nat. Rev. Chem. 2018, 2, 6–14. [Google Scholar] [CrossRef]
  2. Finiels, A.; Fajula, F.; Hulea, V. Nickel-based solid catalysts for ethylene oligomerization-a review. Catal. Sci. Technol. 2014, 4, 2412–2426. [Google Scholar] [CrossRef]
  3. Shin, D.Y.; Yoon, J.H.; Baik, H.; Lee, S.J. A way to avoid polymeric side products during the liquid-phase ethylene oligomerization with SBA-15 supported (bpy)Ni(II)Cl2 heterogeneous catalyst. Appl. Catal. A-G 2020, 590, 117363–117369. [Google Scholar] [CrossRef]
  4. Wang, J.; Alam, F.; Chang, Q.; Chen, Y.; Jiang, T. Catalytic behavior tuning via structural modifications of silylated-diphosphine Ni(II) complexes for ethylene selective dimerization. Appl. Organomet. Chem. 2020, 34, e5722. [Google Scholar] [CrossRef]
  5. Nicholas, C.P.; Laipert, L.; Prabhakar, S. Oligomerization of Light Olefins to Gasoline: An Advanced NMR Characterization of Liquid Products. Ind. Eng. Chem. Res 2016, 55, 9140–9146. [Google Scholar] [CrossRef]
  6. Wang, Z.; Liu, Q.; Solan, G.A.; Sun, W.-H. Recent advances in Ni-mediated ethylene chain growth: Nimine-donor ligand effects on catalytic activity, thermal stability and oligo-/polymer structure. Coordin. Chem. Rev. 2017, 350, 68–83. [Google Scholar] [CrossRef]
  7. Chen, L.; Huo, H.; Wang, L.; Kuang, Q.; Shi, W.; Zhang, N.; Li, Z.; Wang, J. Ethylene oligomerization studies utilizing nickel complexes bearing pyridine-imine ligands. Inorg. Chim. Acta 2019, 491, 67–75. [Google Scholar] [CrossRef]
  8. Feng, C.; Zhou, S.; Wang, D.; Zhao, Y.; Liu, S.; Li, Z.; Braunstein, P. Cooperativity in Highly Active Ethylene Dimerization by Dinuclear Nickel Complexes Bearing a Bifunctional PN Ligand. Organometallics 2020, 40, 184–193. [Google Scholar] [CrossRef]
  9. Olivier-Bourbigou, H.; Breuil, P.A.R.; Magna, L.; Michel, T.; Espada Pastor, M.F.; Delcroix, D. Nickel Catalyzed Olefin Oligomerization and Dimerization. Chem. Rev. 2020, 120, 7919–7983. [Google Scholar] [CrossRef]
  10. Sung Cho, H.; Deng, H.; Miyasaka, K.; Dong, Z.; Cho, M.; Neimark, A.V.; Ku Kang, J.; Yaghi, O.M.; Terasaki, O. Extra adsorption and adsorbate superlattice formation in metal-organic frameworks. Nature 2015, 527, 503–507. [Google Scholar] [CrossRef]
  11. Furukawa, H.; Cordova, K.E.; O’Keeffe, M.; Yaghi, O.M. The chemistry and applications of metal-organic frameworks. Science 2013, 341, 1230444–1230456. [Google Scholar] [CrossRef] [Green Version]
  12. Hanikel, N.; Prevot, M.S.; Yaghi, O.M. MOF water harvesters. Nat. Nanotechnol. 2020, 15, 348–355. [Google Scholar] [CrossRef]
  13. Ji, Z.; Li, T.; Yaghi, O.M. Sequencing of metals in multivariate metal-organic frameworks. Science 2020, 369, 674–780. [Google Scholar] [CrossRef]
  14. Wang, C.; Li, G.; Guo, H. Heterogeneous dimerization of ethylene by coordinatively unsaturated metal sites in two forms of Ni-MIL-77. Mol. Catal. 2022, 524, 112340–112348. [Google Scholar] [CrossRef]
  15. Ma, L.; Falkowski, J.M.; Abney, C.; Lin, W. A series of isoreticular chiral metal-organic frameworks as a tunable platform for asymmetric catalysis. Nat. Chem. 2010, 2, 838–846. [Google Scholar] [CrossRef]
  16. Li, Z.; Schweitzer, N.M.; League, A.B.; Bernales, V.; Peters, A.W.; Getsoian, A.B.; Wang, T.C.; Miller, J.T.; Vjunov, A.; Fulton, J.L.; et al. Sintering-Resistant Single-Site Nickel Catalyst Supported by Metal-Organic Framework. J. Am. Chem. Soc. 2016, 138, 1977–1982. [Google Scholar] [CrossRef]
  17. Hu, Y.; Zhang, Y.; Han, Y.; Sheng, D.; Shan, D.; Liu, X.; Cheng, A. Ultrathin Nickel-Based Metal–Organic Framework Nanosheets as Reusable Heterogeneous Catalyst for Ethylene Dimerization. ACS Appl. Nano Mater. 2018, 2, 136–142. [Google Scholar] [CrossRef]
  18. Mlinar, A.N.; Keitz, B.K.; Gygi, D.; Bloch, E.D.; Long, J.R.; Bell, A.T. Selective Propene Oligomerization with Nickel(II)-Based Metal–Organic Frameworks. ACS Catal. 2014, 4, 717–721. [Google Scholar] [CrossRef] [Green Version]
  19. Canivet, J.; Aguado, S.; Schuurman, Y.; Farrusseng, D. MOF-supported selective ethylene dimerization single-site catalysts through one-pot postsynthetic modification. J. Am. Chem. Soc. 2013, 135, 4195–4198. [Google Scholar] [CrossRef]
  20. Metzger, E.D.; Brozek, C.K.; Comito, R.J.; Dinca, M. Selective Dimerization of Ethylene to 1-Butene with a Porous Catalyst. ACS Cent. Sci. 2016, 2, 148–153. [Google Scholar] [CrossRef] [Green Version]
  21. Chen, C.; Alalouni, M.R.; Dong, X.; Cao, Z.; Cheng, Q.; Zheng, L.; Meng, L.; Guan, C.; Liu, L.; Abou-Hamad, E.; et al. Highly Active Heterogeneous Catalyst for Ethylene Dimerization Prepared by Selectively Doping Ni on the Surface of a Zeolitic Imidazolate Framework. J. Am. Chem. Soc. 2021, 143, 7144–7153. [Google Scholar] [CrossRef] [PubMed]
  22. Yaghi, O.M.; Li, H.; Groy, T.L. Construction of Porous Solids from Hydrogen-Bonded Metal Complexes of 1,3,5-Benzenetricarboxylic Acid. J. Am. Chem. Soc. 1996, 118, 9096–9101. [Google Scholar] [CrossRef]
  23. Naik Shreyanka, S.; Theerthagiri, J.; Lee, S.J.; Yu, Y.; Choi, M.Y. Multiscale design of 3D metal–organic frameworks (M−BTC, M: Cu, Co, Ni) via PLAL enabling bifunctional electrocatalysts for robust overall water splitting. Chem. Eng. J. 2022, 446, 137045. [Google Scholar] [CrossRef]
  24. Du, P.; Dong, Y.; Liu, C.; Wei, W.; Liu, D.; Liu, P. Fabrication of hierarchical porous nickel based metal-organic framework (Ni-MOF) constructed with nanosheets as novel pseudo-capacitive material for asymmetric supercapacitor. J. Colloid Interface Sci. 2018, 518, 57–68. [Google Scholar] [CrossRef] [PubMed]
  25. Wu, Y.; Song, X.; Li, S.; Zhang, J.; Yang, X.; Shen, P.; Gao, L.; Wei, R.; Zhang, J.; Xiao, G. 3D-monoclinic M–BTC MOF (M = Mn, Co, Ni) as highly efficient catalysts for chemical fixation of CO2 into cyclic carbonates. J. Ind. Eng. Chem. 2018, 58, 296–303. [Google Scholar] [CrossRef]
  26. Gan, Q.; He, H.; Zhao, K.; He, Z.; Liu, S. Morphology-dependent electrochemical performance of Ni-1,3,5-benzenetricarboxylate metal-organic frameworks as an anode material for Li-ion batteries. J. Colloid Interface Sci. 2018, 530, 127–136. [Google Scholar] [CrossRef]
  27. Maiti, S.; Pramanik, A.; Manju, U.; Mahanty, S. Reversible Lithium Storage in Manganese 1,3,5-Benzenetricarboxylate Metal-Organic Framework with High Capacity and Rate Performance. ACS Appl. Mater. Interfaces 2015, 7, 16357–16363. [Google Scholar] [CrossRef]
  28. Singh, M.P.; Dhumal, N.R.; Kim, H.J.; Kiefer, J.; Anderson, J.A. Influence of Water on the Chemistry and Structure of the Metal−Organic Framework Cu3(btc)2. J. Phys. Chem. C 2016, 120, 17323–17333. [Google Scholar] [CrossRef]
  29. Sánchez-Andújar, M.; Gómez-Aguirre, L.C.; Pato Doldán, B.; Yáñez-Vilar, S.; Artiaga, R.; Llamas-Saiz, A.L.; Manna, R.S.; Schnelle, F.; Lang, M.; Ritter, F.; et al. First-order structural transition in the multiferroic perovskite-like formate [(CH3)2NH2][Mn(HCOO)3]. CrystEngComm 2014, 16, 3558–3566. [Google Scholar] [CrossRef] [Green Version]
  30. Sun, K.; Li, L.; Yu, X.; Liu, L.; Meng, Q.; Wang, F.; Zhang, R. Functionalization of mixed ligand metal-organic frameworks as the transport vehicles for drugs. J. Colloid Interface Sci. 2017, 486, 128–135. [Google Scholar] [CrossRef]
  31. Zeng, G.J.; Chen, Y.; Chen, L.; Xiong, P.X.; Wei, M.D. Hierarchical cerium oxide derived from metal-organic frameworks for high performance supercapacitor electrodes. Electrochim. Acta 2016, 222, 773–780. [Google Scholar] [CrossRef]
  32. He, J.H.; Zhang, Y.T.; Pan, Q.H.; Yu, J.H.; Ding, H.; Xu, R.R. Three metal-organic frameworks prepared from mixed solvents of DMF and HAc. Micropor. Mesopor. Mat 2006, 90, 145–152. [Google Scholar] [CrossRef]
  33. Israr, F.; Kim, D.K.; Kim, Y.; Oh, S.J.; Ng, K.C.; Chun, W. Synthesis of porous Cu-BTC with ultrasonic treatment: Effects of ultrasonic power and solvent condition. Ultrason. Sonochem. 2016, 29, 186–193. [Google Scholar] [CrossRef]
  34. Xu, J.; Yang, C.; Xue, Y.; Wang, C.; Cao, J.; Chen, Z. Facile synthesis of novel metal-organic nickel hydroxide nanorods for high performance supercapacitor. Electrochim. Acta 2016, 211, 595–602. [Google Scholar] [CrossRef]
  35. Yi, F.Y.; Chen, D.; Wu, M.K.; Han, L.; Jiang, H.L. Chemical Sensors Based on Metal-Organic Frameworks. ChemPlusChem 2016, 81, 675–690. [Google Scholar] [CrossRef]
  36. Xiao, X.; Zhang, G.; Xu, Y.; Zhang, H.; Guo, X.; Liu, Y.; Pang, H. A new strategy for the controllable growth of MOF@PBA architectures. J. Mater. Chem. A 2019, 7, 17266–17271. [Google Scholar] [CrossRef]
  37. Wang, X.; Jian, H.; Xiao, Q.; Huang, S. Ammonium nickel phosphate on nickel foam with a Ni3+-rich surface for ultrasensitive nonenzymatic glucose sensors. Appl. Surf. Sci. 2018, 459, 40–47. [Google Scholar] [CrossRef]
  38. Raihana, M.K.; Padmanathan, N.; Eswaramoorthi, V.; McNulty, D.; Sahadevan, J.; Mohanapriya, P.; Muthu, S.E. Reduced graphene oxide/VSB-5 composite micro/nanorod electrode for high energy density supercapattery. Electrochim. Acta 2021, 391, 138903–138914. [Google Scholar] [CrossRef]
  39. Dilks, A. The identification of peroxy-features at polymer surfaces by ESCA. J. Polym. Sci. Pol. Chem. Edit. 1981, 19, 1319–1327. [Google Scholar] [CrossRef]
  40. Gedrich, K.; Senkovska, I.; Klein, N.; Stoeck, U.; Henschel, A.; Lohe, M.R.; Baburin, I.A.; Mueller, U.; Kaskel, S. A highly porous metal-organic framework with open nickel sites. Angew. Chem. Int. Ed. 2010, 49, 8489–8492. [Google Scholar] [CrossRef]
  41. Maniam, P.; Stock, N. Investigation of porous Ni-based metal-organic frameworks containing paddle-wheel type inorganic building units via high-throughput methods. Inorg. Chem 2011, 50, 5085–5097. [Google Scholar] [CrossRef] [PubMed]
  42. Tian, F.; Ru, Q.; Qiao, C.; Sun, X.; Jia, C.; Wang, Y.; Zhang, Y. Adsorption desulfurization of model gasoline by metal–organic framework Ni3(BTC)2. J. Energy Chem. 2019, 32, 8–14. [Google Scholar] [CrossRef] [Green Version]
  43. Israr, F.; Kim, D.K.; Kim, Y.; Chun, W. Scope of various solvents and their effects on solvothermal synthesis of Ni-BTC. Quim. Nova 2016, 39, 669–675. [Google Scholar] [CrossRef]
  44. Murad, A.; Liew, J.Y.C.; Yaacob, M.H.; Noor, I.M.; Osman, N.H.; Kamarudin, M.A.; Tan, S.T.; Lee, H.K.; Talib, Z.A.; Alresheedi, M.T.; et al. Effect of nickel ion concentration on structural, optical and electrical properties towards Ni–H3BTC-MOF formation for nonlinear saturable absorption phenomenon. J. Phys. Chem. Sol. 2022, 167, 110743–110751. [Google Scholar] [CrossRef]
  45. Zhang, Y.; Liu, Z.; Guo, C.; Chen, T.; Guo, C.; Lu, Y.; Wang, J. CdS(ZB)/CdS(WZ)/Ni-BTC photocatalytic selective oxidation of benzyl alcohol to benzaldehyde coupled with hydrogen evolution. Appl. Surf. Sci. 2022, 571, 151284–151296. [Google Scholar] [CrossRef]
  46. Taherinia, D.; Hatami, H.; Mirzaee Valadi, F. Trimetallic Co-Ni-Mn metal-organic framework as an efficient electrocatalyst for alkaline oxygen evolution reaction. J. Electroanal. Chem. 2022, 922, 116720–116729. [Google Scholar] [CrossRef]
  47. Israr, F.; Chun, D.; Kim, Y.; Kim, D.K. High yield synthesis of Ni-BTC metal-organic framework with ultrasonic irradiation: Role of polar aprotic DMF solvent. Ultrason. Sonochem. 2016, 31, 93–101. [Google Scholar] [CrossRef]
  48. Nyamato, G.S.; Alam, M.G.; Ojwach, S.O.; Akerman, M.P. (Pyrazolyl)-(phosphinoyl)pyridine iron(II), cobalt(II) and nickel(II) complexes: Synthesis, characterization and ethylene oligomerization studies. J. Organomet. Chem. 2015, 783, 64–72. [Google Scholar] [CrossRef]
  49. Rhinehart, J.L.; Brown, L.A.; Long, B.K. A robust Ni(II) alpha-diimine catalyst for high temperature ethylene polymerization. J. Am. Chem. Soc. 2013, 135, 16316–16319. [Google Scholar] [CrossRef]
  50. Andrei, R.D.; Popa, M.I.; Fajula, F.; Hulea, V. Heterogeneous oligomerization of ethylene over highly active and stable Ni-AlSBA-15 mesoporous catalysts. J. Catal. 2015, 323, 76–84. [Google Scholar] [CrossRef]
  51. Chen, L.; Jiang, Y.; Huo, H.; Liu, J.; Li, Y.; Li, C.; Zhang, N.; Wang, J. Metal-organic framework-based composite Ni@MOF as Heterogenous catalyst for ethylene trimerization. Appl. Catal. A-G 2020, 594, 117457–117465. [Google Scholar] [CrossRef]
  52. Brogaard, R.Y.; Olsbye, U. Ethene Oligomerization in Ni-Containing Zeolites: Theoretical Discrimination of Reaction Mechanisms. ACS Catal. 2016, 6, 1205–1214. [Google Scholar] [CrossRef]
  53. Moussa, S.; Concepción, P.; Arribas, M.A.; Martínez, A. The nature of active Ni sites and the role of Al species in the oligomerization of ethylene on mesoporous Ni-Al-MCM-41 catalysts. Appl. Catal. A-G 2020, 608, 117831–117841. [Google Scholar] [CrossRef]
  54. Lever, A.B.P.; Lewis, J.; Nyholm, R.S. Pyraxine Metal Complexes. Part III.* Derivatives of Nickel (II). J. Chem. Soc. 1963, 1, 5042–5048. [Google Scholar] [CrossRef]
  55. Wu, J.X.; Yuan, W.W.; Xu, M.; Gu, Z.Y. Ultrathin 2D nickel zeolitic imidazolate framework nanosheets for electrocatalytic reduction of CO2. Chem. Commun. 2019, 55, 11634–11637. [Google Scholar] [CrossRef]
  56. Jafari, N.; Zeinali, S.; Shadmehr, J. Room temperature resistive gas sensor based on ZIF-8/MWCNT/AgNPs nanocomposite for VOCs detection. J. Mate. Sci.-Mater. El 2019, 30, 12339–12350. [Google Scholar] [CrossRef]
  57. Borges, W.M.S.; Guerreiro, M.C.; Anconi, C.P.A.; Magalhães, K.T.; Castro, G.M.M.; Neto, J.L.; Rossi, M.A.L.S. Coordination of iron (III) to modified silica surface containing pyrazine acid groups and its application in advanced oxidative processes. Surf. Interfaces 2022, 29, 101770–101779. [Google Scholar] [CrossRef]
  58. Sun, X.; Man, J.; Liu, K.; Liu, W.; Sun, J.; Zhang, N.; Zhou, Y.; Geng, Z.; Li, S.; Sun, J. Uniform lithium deposition enabled by a carbon nanotubes framework modified with nanosized ZIF-8 particles for dendrite-free lithium metal anode. Appl. Surf. Sci. 2023, 616, 156474–156484. [Google Scholar] [CrossRef]
  59. Mohammadi, A.; Nakhaei Pour, A. Triethylenetetramine-impregnated ZIF-8 nanoparticles for CO2 adsorption. J. CO2 Util 2023, 69, 102424–102437. [Google Scholar] [CrossRef]
  60. Zhang, Z.; Chen, Y.; Hu, C.; Zuo, C.; Wang, P.; Chen, W.; Ao, T. Efficient removal of tetracycline by a hierarchically porous ZIF-8 metal organic framework. Environ. Res. 2021, 198, 111254–111266. [Google Scholar] [CrossRef]
  61. Chen, C.; Alalouni, M.R.; Xiao, P.; Li, G.; Pan, T.; Shen, J.; Cheng, Q.; Dong, X. Ni-Loaded 2D Zeolitic Imidazolate Framework as a Heterogeneous Catalyst with Highly Activity for Ethylene Dimerization. Ind. Eng. Chem. Res. 2022, 61, 14374–14381. [Google Scholar] [CrossRef]
  62. Li, D.; Li, F.; Yu, H.; Guo, L.; Huang, J.; Li, J.; Li, C. Nickel-modified triphenylamine-based conjugated porous polymers as precatalyst for ethylene oligomerization. Inorg. Chim. Acta 2023, 544, 121228–121238. [Google Scholar] [CrossRef]
  63. Li, D.; Guo, L.; Li, F.; Huang, J.; Li, J.; Li, M.; Li, C. Synthesis and catalytic behavior of nickel heterogenized in covalent organic frameworks as precatalysts in ethylene oligomerization. Micropor. Mesopor. Mat. 2022, 338, 111979–111992. [Google Scholar] [CrossRef]
  64. Metzger, E.D.; Comito, R.J.; Wu, Z.; Zhang, G.; Dubey, R.C.; Xu, W.; Miller, J.T.; Dincă, M. Highly Selective Heterogeneous Ethylene Dimerization with a Scalable and Chemically Robust MOF Catalyst. ACS Sustain. Chem. Eng. 2019, 7, 6654–6661. [Google Scholar] [CrossRef]
  65. Liu, B.; Jie, S.; Bu, Z.; Li, B.-G. Postsynthetic modification of mixed-linker metal–organic frameworks for ethylene oligomerization. RSC Adv. 2014, 4, 62343–62346. [Google Scholar] [CrossRef]
Figure 1. Probable tube view of nickel atoms in their environment with NiBTCs (Red circles indicated coordination water molecules) [26,27].
Figure 1. Probable tube view of nickel atoms in their environment with NiBTCs (Red circles indicated coordination water molecules) [26,27].
Catalysts 13 00640 g001
Figure 2. (A) XRD patterns of NiBTC–DMF (blue) and NiBTC–EtOH (red); (B) FT-IR spectra of NiBTC–DMF (blue) and NiBTC–EtOH (red). (C) FT-IR spectra of NiBTC–DMF (blue) and NiBTC–EtOH (red) at 1800–1200 cm−1.
Figure 2. (A) XRD patterns of NiBTC–DMF (blue) and NiBTC–EtOH (red); (B) FT-IR spectra of NiBTC–DMF (blue) and NiBTC–EtOH (red). (C) FT-IR spectra of NiBTC–DMF (blue) and NiBTC–EtOH (red) at 1800–1200 cm−1.
Catalysts 13 00640 g002
Figure 3. XPS patterns of NiBTC–DMF (blue) and NiBTC–EtOH (red): (A) survey, (B) Ni 2p, (C) C 1 s and (D) O 1 s.
Figure 3. XPS patterns of NiBTC–DMF (blue) and NiBTC–EtOH (red): (A) survey, (B) Ni 2p, (C) C 1 s and (D) O 1 s.
Catalysts 13 00640 g003
Figure 4. TGA curves (A,B) and N2 adsorption-desorption isotherms of NiBTCs (C).
Figure 4. TGA curves (A,B) and N2 adsorption-desorption isotherms of NiBTCs (C).
Catalysts 13 00640 g004
Figure 5. (A) Effect of Al/Ni; (B) Effect of temperature and (C) Effect of the amounts of catalyst on the catalytic activity and the product distribution. Reaction conditions: Ethylene pressure of 10 bar, 0.5 h, 400 rpm, NiBTC–DMF activated by 150 °C and Et2AlCl as a co-catalyst.
Figure 5. (A) Effect of Al/Ni; (B) Effect of temperature and (C) Effect of the amounts of catalyst on the catalytic activity and the product distribution. Reaction conditions: Ethylene pressure of 10 bar, 0.5 h, 400 rpm, NiBTC–DMF activated by 150 °C and Et2AlCl as a co-catalyst.
Catalysts 13 00640 g005
Figure 6. (A) Postulated catalytic cycle for ethylene dimerization by NiBTCs; (B) Chromatogram of the products after ethylene dimerization with NiBTC–EtOH for 1 h.
Figure 6. (A) Postulated catalytic cycle for ethylene dimerization by NiBTCs; (B) Chromatogram of the products after ethylene dimerization with NiBTC–EtOH for 1 h.
Catalysts 13 00640 g006
Figure 7. (A) XRD patterns of Ni(pyz)2Cl2 (green) and α–Ni(im)2 (purple); (B) FT–IR spectra of Ni(pyz)2Cl2 (green) and α–Ni(im)2 (purple); (C) FT–IR spectra of Ni(pyz)2Cl2 (green) and α–Ni(im)2 (purple) at 1800–1200 cm−1.
Figure 7. (A) XRD patterns of Ni(pyz)2Cl2 (green) and α–Ni(im)2 (purple); (B) FT–IR spectra of Ni(pyz)2Cl2 (green) and α–Ni(im)2 (purple); (C) FT–IR spectra of Ni(pyz)2Cl2 (green) and α–Ni(im)2 (purple) at 1800–1200 cm−1.
Catalysts 13 00640 g007
Scheme 1. Schematic illustration describing the synthesis of NiBTC–DMF and NiBTC–EtOH.
Scheme 1. Schematic illustration describing the synthesis of NiBTC–DMF and NiBTC–EtOH.
Catalysts 13 00640 sch001
Scheme 2. Schematic illustration describing the synthesis of Ni(pyz)2Cl2.
Scheme 2. Schematic illustration describing the synthesis of Ni(pyz)2Cl2.
Catalysts 13 00640 sch002
Scheme 3. Schematic illustration describing the synthesis of α–Ni(im)2.
Scheme 3. Schematic illustration describing the synthesis of α–Ni(im)2.
Catalysts 13 00640 sch003
Table 1. Ethylene dimerization with NiBTCs.
Table 1. Ethylene dimerization with NiBTCs.
CatalystTime
(h)
Ethylene Pressure
(bar)
Activity
gpro./(gcat.·h)
TOF
(h−1)
Selectivity (%)
1-C4Other C4C6≥C8
Ni(NO3)2 6H2O + H3BTC + Et2AlCl0.510000000
H3BTC + Et2AlCl0.510000000
NiBTC–DMF0.510196.9132586.59.401.302.80
1.010157.2105776.916.52.304.30
0.520470.9316783.28.302.515.99
NiBTC–EtOH0.510291.6176478.016.91.553.55
1.010279.4169177.914.72.874.53
0.520647.0391581.712.32.763.24
Reaction conditions: 50 °C, 400 rpm, 0.005 g NiBTCs activated by 150 °C, Al:Ni = 100, Et2AlCl as a co-catalyst.
Table 2. Comparison of the amount of product obtained from the leaching test.
Table 2. Comparison of the amount of product obtained from the leaching test.
EntryAmount of Product Obtained (g)Amount of Product Obtained from the Filtrate (g)
NiBTC–DMF0.4920.009
NiBTC–EtOH0.7290.035
Leaching test conditions: Ethylene pressure of 10 bar, 400 rpm, NiBTC activated by 150 °C and Et2AlCl as a co-catalyst, 0.5 h.
Table 3. Ethylene dimerization with recovered NiBTCs.
Table 3. Ethylene dimerization with recovered NiBTCs.
EntryNi Content % aAl Content % aActivity gpro./(gcat·h)TOF (h−1)Selectivity (%)
1-C4Other C4C6≥C8
NiBTC–DMF–R20.897.54106.2714.385.14.310.3910.2
NiBTC–EtOH–R24.776.54121.0732.174.911.31.3012.5
Reaction conditions: Ethylene pressure of 10 bar, Al:Ni = 100, 50 °C, 0.5 h, 400 rpm, 0.005 g NiBTC activated by 150 °C and Et2AlCl as a co-catalyst. a Measured by ICP-OES at the same concentration (0.001 g/L).
Table 4. Comparison of catalytic performance of Ni-MOFs in ethylene dimerization.
Table 4. Comparison of catalytic performance of Ni-MOFs in ethylene dimerization.
EntryActivity gpro./(gcat.·h)TOF (h−1)Selectivity (%)
1-C4Other C4C6≥C8
NiBTC–DMF196.9132586.59.401.302.80
NiBTC–EtOH291.6176478.016.91.553.55
Ni(pyz)2Cl2149.7126179.112.20.787.92
α–Ni(im)2184.7107571.918.71.787.62
Reaction conditions: Ethylene pressure of 10 bar, Al:Ni = 100, 50 °C, 0.5 h, 400 rpm, 0.005 g catalyst activated by 150 °C and Et2AlCl as a co-catalyst.
Table 5. Comparison of reported catalytic activity of Ni–MOFs for ethylene dimerization.
Table 5. Comparison of reported catalytic activity of Ni–MOFs for ethylene dimerization.
EntryEthylene Pressure
(bar)
Al/Ni Molar RatioActivity gpro./(gcat.·h)Selectivity of 1-C4 (%)Ref.
Ni–ZIF–8504640213085.1[21]
45 Ni–ZIF–L30718771.9686.3[61]
Ni@TAPA–CPPs5500251.9229.6[62]
Ni@MAPA–COF7500202.5147.5[63]
Ni@MOF1080043.5243.7[51]
30Ni@(Fe)–MIL–1013070205.0Not report[19]
Ni(1%)–MFU–4l50500198.092.0[20]
Ni(7.5%)–CFA-150200022.2387.1[64]
IRMOF–3–Ni20100125.835.0 (C4 %)[65]
MixMOF–Ni-b20100492.992.7 (C4 %)[65]
NiBTC–DMF20100470.983.2This work
NiBTC–EtOH20100647.081.7This work
Table 6. The yields of the Ni-MOFs and nickel content.
Table 6. The yields of the Ni-MOFs and nickel content.
EntryYield %Content of Ni wt.% a
NiBTC–DMF56.0831.16
NiBTC–EtOH65.6334.64
Ni(pyz)2Cl250.3819.68
α–Ni(im)241.2228.47
a Measured by ICP–OES.
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Wang, C.; Li, G.; Guo, H. Ethylene Dimerization Performance of NiBTCs Synthesized Using Different Solvents. Catalysts 2023, 13, 640. https://doi.org/10.3390/catal13030640

AMA Style

Wang C, Li G, Guo H. Ethylene Dimerization Performance of NiBTCs Synthesized Using Different Solvents. Catalysts. 2023; 13(3):640. https://doi.org/10.3390/catal13030640

Chicago/Turabian Style

Wang, Cong, Gang Li, and Hongchen Guo. 2023. "Ethylene Dimerization Performance of NiBTCs Synthesized Using Different Solvents" Catalysts 13, no. 3: 640. https://doi.org/10.3390/catal13030640

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop