Location via proxy:   [ UP ]  
[Report a bug]   [Manage cookies]                

A21

Download as pdf
Download as pdf
You are on page 1of 9
ap Designation: A 21 - 94 Standard Specification for Carbon Steel Axles, Non-Heat-Treated and Heat-Treated, for Railway Use' ‘Trig standard i issued under the fined designation A721; he number immdaely folowing th designation indiaes he yen of iil adoption cn the ae of ison the yar ot ein. A nuabe in pareateses cae he ea fa enrol. A ‘percept epson idaies an cil change since the as esi 0 approval 1, Scope LL This specification covers nonheat-treated axles up 10 and including those 62 in. (165.1 mm) nominal diameter at the center and heat-treated axles of all sizes for freight cars, passenger cars, and locomotives. 1.2 This specification is for axles with machined bodies. For axles with as-forged bodies, see Specification A 383. 1.3 The grades of carbon steel axles are as follows: 13.1 Grade U—Nonheat-treated. 3.2 Grade F—Double normalized and tempered. (Al! freight axles over 6% in. (165.1 mm) nominal diameter at the center shall be Grade F.) 1.33 Grade G—Quenched and tempered 1.34 Grade H—Normalized, quenched, and tempered. 3.5 Grades F, G, and H axles are used in heavy-duty service on locomotives, cars, and other equipment. 1.4 Typical designs for plain and rolier bearing axles are shown in the Manual of Standards and Recommended Practice of the Association of American Railroads 1.5 Supplementary requirements are provided for use when additional testing or inspection is desired. These shall apply only when specified individually by the purchaser in the order. 1.6 The values stated in inch-pound units are 10 be regarded as the standard 2. Referenced Documents 2.1 ASTM Standards: A370 Test Methods and Defi Testing of Steel Products? ‘A383 Specification for Axles, Railway, Carbon Steel, Untreated for Export and General Industrial Use* E 112 Test Methods for Determining Average Grain Size* E 127 Practice for Fabricating and Checking Aluminum Alloy Ultrasonic Standard Reference Blocks E381 Method of Macroetch Testing Steel Bars, Billets, Blooms, and Forgings? 2.2 Mititary Standards. ns for Mechanical his spciestion suerte srnicion of ASTM Commie AI on Stes ‘Staines Steel ana Related! Aly and he dt esponsitty of Subcom nee ‘A007 on Sis! Wheel, Tres and Forgings for Rata Serve. Curt edition apptoved Feb. 18, 1998, Published April 1994, Originally pushed 1s A21~ 800 T Last previous edition &20~88 2Ontzinable rom De Mechaneal Division, Auocation of American Rall roads 1920 1 Su 94, Wharton, De 20036, "nal Book of ASTM Standard, Vol 01.03, saa! Boot of ASTM Standard, Vol 01.34 > anneal ook of ASTM Stondards, Val D301 ual Book of ASTM Standard, Vol 03.03 ‘MIL-STD-29 Marking for Shipment and Storage? MIL-STD-I63 Steel Mill Products, Preparation for Ship- ment and Storage” 2.3 Federal Standard: Fed, Std. No. 123 Marking for Shipments (Civil Agencies)? 3. Ordering Information 3.1 The inquiry, order, or contract for material under this specification shall include the following information 3.1.1 Quantity (number of pieces), 3.1.2 ASTM designation and year of issue, 3.1.3 Grade, 3.1.4 Design and size, 3.1.5 Intended service, and 3.1.6 Supplementary requirements (if any), 4. Manufacture 4.1 Process—The steel shall be made by any of the following processes: open-heasth, electric-furnace, or basic~ oxygen, 4.2 Discard—Sulficient discard shall be made to assure freedom from piping and undue segregation, 4.3. Forging Practice—The axles may be made direct from the ingot or from blooms. The total reduction from ingot or strand cast bloom to forging shall not be less than 3 t0 1, unless otherwise specified 4.4 Cooling and Heating: 4.4.1 Afier axle biooms are produced they shall be slow cooled in closed containers, hoods, or furnaces. 4.4.2 Blooms shall be reheated for forging in a manner ‘which will prevent internal bursts and overheating. 4.4.3 After forging, axles shall be slow cooled in closed containers, covered conveyors, or in hoods. If axles (Grades F, G, and H) are heat-treated directly from the forging, they shall be slow cooled following the final heat treatment. Note 1—After slow cooling, Grade U axles may be single normal ized in accordance with 4.44 and 4.3.2 4.4.4 Axles (Grades F, G, and H) that are heat-treated directly from forging (1) shall be cooled below the transfor- mation temperature or to approximately 1000°F (538°C) before any reheating operation and (2) must not be per= mitted 10 coo! below S00°F (260°C) without slow cooling as defined in 4.4.3. Note 2—-As the temperature of the sales approaches the minimum ‘of SOO'F (260°C) a supplemental heat source may be necestary 10 are fn elective slow cooling evete ” avalbe from Standardization Documents Order Desk, Edy. 4 Section D, 100 Robbins Ave, Phihdeptia, Pa 191113094, Auta’ NPODS ah az TABLE 1 Chemica! Requirements I caroosten erent |__Tnald losiiianal ea ow [oak os | ome formes | 050 | 090. 080 | 980. | aso | aso promo aes Sous oes cue eso | Sone ose Secon ais ais 4.4.5 When properly vacuum-degassed steel is used, the slow cooling requirements of 4.4.1, 4.4.3, and 4.4.4 may be ‘omitted but axle blooms must then be pile cooled. 4.5 Heat Treatment: 4.3.1 Axles for heat treatment shall be reheated gradually and uniformly to a suitable temperature to refine the grain structure. 4.5.2 Normalizing—After beating to a suitable tempera- ture the axles shall be withdrawn from the furnace and allowed to cool in air. A furnace charge thus treated is called 2 normalizing charge. Cooling may be accelerated by in- creased air circulation which must be controlled to provide reasonably uniform cooling. 4.5.3 Double Normalizing—The procedure shall consist of two separate normalizing treatments, The second shall be performed at a lower temperature than the first treatment. A furnace charge thus treated is termed a double-normalizing charge. Cooling may be accelerated by increased air circula- tion which must be controlled to provide reasonably uniform cooling. Nove 3—A single notmalizing eatment shall be permited when all other requirements for Grade F are met 4.54 Quenching—Aficr heating to a suitable temperature the axles shall be quenched in @ suitable medium under reasonably uniform conditions. A furnace charge thus treated is termed a quenching charg. 4.55 Fempering—Aales shall be reheated gradually to, ‘and held zt, a suitable temperature below the critical range ‘and shall then be allowed to cool under suitable conditions, ‘A furnace charge thus treated is termed a tempering charge. 4.5.6 Heat treatment may be performed in either baich- type furnaces or continuous furnaces 46 Straightening. 4.6.1 Any straightening of axle forgings shall be done before machining and in such 2 manner as to leave the axie body free of injurious marks. 462 Straightening shall preferably be performed at a temperature no lower than 950°F (510°C). Straightening performed at_a temperature lower than 950°F shall be followed by a furnace stress-relieving procedure or applicable heat treatment. 5. Chemical Requirements 5.1 Chemical Composition—The steel shall conform {o the requirements for chemical composition shown in Table 1 5.2 Cast or Heat Analysis—An analysis of each cast or hheat shall be made by the manufacturer to determine the ‘TABLE 2 Permissible Variations for Product Analyse (for Cross ‘Section 100 In. (645 cm*) and Under) Nove—Prodict coss-sectoral aoa deed 8s eer (@) asim conection wea ot ‘Area takan aight anges othe |i of he onghat ingot or bet arent ‘Mauri Lint or Ure =~ met Prasrons 2.008 eur 2.008 ‘Sie 992 percentages of the elements specified in Table |. The analysis. shall be made from a test sample taken preferably during the pouring of the cast or heat, The chemical composition thus determined shall conform to the requirements in Table 1. 5.3 Product Analysis—An analysis may be made by the purchaser from one axle representing each heat. The chem- ical composition thus determined shall conform to the requirements of 5.1 subject to tolerances included in Table 2. ‘The sample for these analyses shail be taken from one end of the test axle or full-sized prolongation at a point midway between the center and surface. If drillings are taken, they shall be obtained using a %s-in, (16-mm) diameter drill or ‘turnings may be taken from a tension test specimen. Mechanical Requirements and Tests for Nonheat-Treated Axles 6. Atthe option of the manufacturer, either drop tests or tension tests (but normally not both) shall be performed to ‘qualify each heat of steel, 62 Drop Tes. 6.2.1 The test axle shall be so placed on supports 3 (914 mm) apart that the tup will strike it midway between the ‘ends. It shall stand without fracture five blows from a tup of 2240 tb (1016 kg) falling from a height H such that AY in feet ‘equals the square of the diameter of the axle at the center in inches, H = d®, The axles shall be rotated through 180° after the first and third blows. 6.2.2 Before the axle is drop tested, the center shall be calipeted 10 the nearest “in. (3.2 mm) and the height of drop in feet, to the nearest Ys fi, shall not be less than the square of the actual diameter at the center in inches. 6.2.3 The permanent set produced by the frst blow shall ‘not exceed that given by the following equation in wiiich L = length of axle in inches and d = diameter of axle at center in inches: Permanent set, max in. LjI.9d~ d+ ve 6.24 The drop test requirements for AAR untreated standard plain bearing axles Classes A to E are shown in Table 3. Drop test requirements for AAR standard roller bearing axles, Classes B to E, are shown in Table 4. Class F and all other plain or roller bearing axles over 6% in. nominal diameter at center are not subject to drop test (ection 1). 6.2.5 The permanent set is the difference between the qb azt TABLE 3. Drop Test Requirements for AAR Plain Boaring Axion Nae aan 7 Legolas, Hegirt Op. Nuno sar aes 8 a aourat nom) fern ‘im tone Pema Se z eT we TTD Dance mean wae 5 Beceem oaon) Bem ower ° 44098 (100.09 2082) ng eon vy zeae) 5 ra Go05) #20238) Bare) recian3y e sty 91270672200) 5989) oss, Bese s bn ts98) Sacer a) scisan ° sity 101128709256) Sane sare 20 escasy 5 Sco97) some sacs su(33 : sey naseey 279 Bneces) sox 2008) tices) 5 becane) gmecies) S0r aon, F 75091210651 9 3048) fone 6 To eatra onan wane TABLE 4 Drop Tost Requiromants for AAR Ft Tae Aan Langinoale, Haga Orp, Namba AAR. ‘oft ffm) mt mae Sm, rome = Tiny a aE a8 wa ciaa wai) aoe 3 esa? 3 tata39) Bac) rater © avy 9270092200) set383) eo 2188) Bas 5 ose, Sagan Bein Sie neoay ° svnby 101198709254) Paces} eve eacasy s aes) Sasa seco Braet € ‘ty 111822704) siete) en e205) Sr 2es) 5 fanaa} pune soa oan F Sey 121661 by 4 woos 6 Teer pone beta distance from a straightedge to the middle point of the axle, ‘measured before the first blow and distance measured in the same manner after the blow. The straightedge shall rest on the end collars or ends of the axle. 6.2.6 The temperature ofthe test axle shalt be between 40 and 120°F (4 and 470), 6.2.7 Ifa drop test axle fails, a retest shall be permitted when it can be determined that the faiture is eaused by a ‘mechanical condition of the drop-est machine (this condi- tion must be corrected before a retest can be performed) or ‘when it can be determined a mechanical flaw in the test axle was the reason for failure 6.28 Drop-Test Machine—The anvil of the drop-test machine shall be supported on twelve springs, as shown in the AAR drawings,’ shall be free to move in a vertical direction, and shall weigh 17 500 Ib (7938 kg). The radius of the striking face of the tup and of the supports shall be 5 in 27 mm). 6.2.9 Number of Drop Tests—One axle, selected by the purchaser's inspector from each heat of steel, shall be drop tested; or the manufacturer may furnish a report of a drop test made previously on the same heat 6.2.10 The manufacturer may substitute Grade F for Grade U axles. Such axles must be marked Grade F and comply with specification requirements for Grade F axles. 6.3 Tension Tests: 6.3.1 Grade U axles (AAR classes B through E) shall be held pending tensile test results and be released if the results conform to Table 6 6.32 The yield point in Table 6 for Classes B through E "Section of the AAR Mechanical Divison Manual of Standards and Recommends Pree Foca 2 ‘may be determined as outlined in 7.1.4 6.3.3 Tension test specimens shall be procured as indi- cated in 7.1.7, 6.3.4 One tension testis required for each untreated heat of axles for qualification of the heat, 6.3.5 If the results of the tension test do not conform to the requirements specified because a flaw developed in the test specimen during testing, a retest is permitted as indicated in 9.1 6.3.6 Ifthe results of the mechanical tests of any Grade U lot of axles do not conform to the requirements specified, the axle having the prolongation from which the tension spec- imen was taken will be drop tested. Failure of the drop test axle is covered in 6.2.7. 7. Mechanical Requirements and Tests for Heat Treated Axles 7.1 Tension Tests 7.1.1 Grades F, G, and H axles shall conform to the requirements in Table 5. 7.1.2 The classification of axle forgings by size shall be determined by the finished diameter of the journal. 7.1.3 The diameter of the test prolongation of axle forgings shall be determined by the forged diameter of the journal. 7.1.4 The yield point in Table 5 for Grade F may be deterrained by the drop of the beam or halt of the gage of the testing machine or, by use of dividers. Where a definite yield point is not exhibited, the yield point method in 7.1.5 shall be used. 7.1.5: The yield point prescribed in Table 5 for Grades G and Hi axles shall be determined by a strain gage or haat TABLE 5 Tensile Requirements for Carbon Stoel Hoat-Treated Axion ‘ean, Seed Dara Tienes" enatesuoagn.min Yak Pit ia eausion of aot ove Net Over 2S ea, mi. __ * om a) ow F ecutieeoatzee are 2 m3 oo 6 som a tree ots 00 © 398” % 2 St Oe So S808 mo 3 Glqvnchad ad tong 4 i02 ooo 20S mt 3 eh Se 7 i a5 000385 SOS 3° 7 1% Be eo 585 SOAS 7 @s 37 aeons 3 *nomatzed euerenes 7 i Ws) 0am BaD 3 tra eere, 7 me 0 eta ome ag AAS % 400 000600 SO.OOO 3 Tears extensometer reading to 0.0002 in. (0.005 mm). Yield point may be defined as the stress at 0.6 % total strain under load for as the stress at 0.2% offset. The method described in Methods and Definitions A 370 shall be followed. After the yield point has been passed the extensometer may then be removed and the test continued to determine the tensile strength. 7.1.6 Tests shall be made only after final heat treatment. TAT Tension Test Specimens 7.1.7.1. Tension test specimens shall be taken from the test, prolongation or an axle in accordance with the provision in 72. 7.17.2 Unless otherwise specified, the axis of the spec imen shall be located et any point midway between the center and surface of the axle or full-sized prolongation and shall be paralle! to the axis of the axle. 7.1.7.3 The tension test specimen shall be machined to the form and dimensions shown in Fig. 5 of Methods and Definitions A 370 covering the standard round tension test specimen with a 2-in. (50.8-mm) gage length 1.2 Prolongation for Test: 7.2.1 For test purposes, prolongations shall be attached to at least $.% of the axles in each size classification of each heat in each heat-treating lot 7.2.2 If axles with prolongations have been expended then axles may be uscd for test procurement. 4,3, Microscopical Tesi—For heat-treated axles (Grades F, G, and H): 7.3.1 A specimen, representing each size classification of each beat in each heat-treatment lot, shall be taken for microscopical test from the tension test specimen. This section for microscopical test shall be cut fom the large tndistorted portion of the tension test specimen in such & ‘way as will give a face transverse to the axis of the axle. 7.3.2 The face shall be polished practically free of seratches and shall be etched to define the microstructure, ‘TABLE 6 Toneiie Requirements For Nonhoat- Treated Axles ‘The specimen shall be examined under a magnification of 100 diameters, 7.3.3 The entire specimen shall show 2 uniform, fine- grained structure, and shall have a grain size of 5 or finer as, ‘measured in accordance with Test Methods E 112, 74 Number of Tests: 7.4.1 Unless otherwise specified by the purchaser, me- ‘chanical tests for grades and sizes shown in Table 5 shall be made upon heat-treated axles as covered in 7.4.2 and 7.4.3, 7.4.2 Where batch-type furnaces are used, one test per grade per heat per size classification is required, but each test shall represent no more than 70 axles. The axles represented by this test shall be called a heat-treatment lot 7.4.3 Where continuous heat-treating furnaces are used, cone test per grade per heat per size classification is required, ‘but each test shall represent no more than 70 axles. The axles represented by this test shall be called a heat-treatment lot 744 If any test specimen fails because of a mechanical condition of the testing apparatus it may be discarded and another specimen taken, 8. Ultrasonic Inspection 8.1 Equipment: 8.1.1 Equipment shall be as follows: 8.1.1.1 The instrument used must be a pulse echo type. 8.1.1.2 The instrument shall be operated at a 2Vi-MHz frequency for both penetrability and discontinuity detection for heat-treated, and at | MHz for nonheat-treated axles. 8.1.1.3 The instrument may use various transducers, ‘namely, quartz | in. (25.4 mm) square or 1% in, (28.6 mm) round, or barium titanate % in. (19.1 mm) to | in. round. ‘The transducer type is at the option of the axle manufac- turer. Other transducers of similar response capability as those described may be used. 8.2 Time of Inspection—Inspection shall be made after axle ends are machined and centered, or at any subsequent stage of processing. 8.3 Instrument Sensitivity and Scanning: 823.1 Irstrument Sensiiny 83.1.4 The instrument sensitivity shall be adjusted to produce an indication of the amplitude specified below, from a reference test block manufactured from a Grade F axle forging having a %4-in, (3.18-mm) diameter, 1-in. (25.4-mm) deep, Nat-bottom hole drilled pexpendiculary to and at a haat distance of 15 in. (381 mm) from the test end face of the axle section. The reference test blocks shall have a surface finish of 80 to 125 pin. (2.03 to 3.18 pm). Alternate references that ive equivalent sensitivity may be used as defined in B.5.1. Indoation Ample, SSH Heat rated anes 2» [Nowbesetened axles * 8.3.1.2 At the sensitivity established in 8.3.1.1 the instru- ment shall detect in reference axles, either heat-treated or nonheat-ireated, a flat-bottom hole of the size and distance specified in the table below. ‘Minimum Size (Fst-Bottom Holes) Detectable {at Various Distances from: End Faces Te te Tet Dance Distance iste eis Stat over 30 moa in oa moe mm) te mm mm Heated ales, in in win Git) G3Sam) Ome Nonbeaeeated as vi "win ‘in (35mm) GSEmm 1805 rm) 83.2 Scanning. 832.1 Scanning shall be performed from both end faces, which shall have a surface finish not exceeding 125-pin G.18-um) finish. The scanning shall include the maximum end face area obtainable by manual or automated inspection, 8.32.2 During scanning the amplitude of the indication from the end face opposite the search unit shall be monitored ‘and the amplitudes of all discontinuity indications shall be evaluated with respect to the distance from the test surface (Gee 8.3.3 and 8.5.2) 8.3.3 Distance-Amplitude Correction—The amplitude of an ultrasonic indication must be considered in relation to its surface to evaluate its significance. This can be accomplished by an electronic device or by distance - amplitude curves (DAC), which are described in 85.2 8.4 Rejection 84.1 Longitudinal Penetration—Axles that do not. pro- duce a 40% FSH minimum back reflection from the end face ‘opposite the search unit shall be rejected or made acceptable by heat treatment. 8.4.2 Discontinuity Test—The aale shall be rejected if the amplitude of any discontinuity indication exceeds the indi- cation levels obtained from the flat-bottom holes listed in the table under 8.3.1.2, considering the distance - amplitude correction as described in 8.3.3 8.5 Additional Information: 85,1 Alternative Reference Standards—Aliernative refer ences may be used 10 establish the test sensitivity if they are cross referenced with the reference test block described in 8.3.1.1. For example, alternative references for heat-treated ¢ equivalent sensitivity: (1) a 1-in. (25.4-mm) indication from a No. | series “A” Alcoa block, and (2) a in, G8.1-mm) indication from an ASTM Practice E 127 block No. 1-0300. 8.5.2 Distance-Amplitule Correction—The ampli ‘an Ultrasonic indication from a given discontinui ide of varies with its distance from the test surface. To compensate for this effec, a distance-amplitude relationship is empioyed. ‘The relationship can be established by an electronic device or by curves. Because the distance-amplitude relationship is influenced primarily by the ultrasonic transducer and instru- ment, it is necessary to relate this factor to the specific ‘equipment used, Appropriate distance-amplitude curves shall be developed. Typical examples are shown in Figs. 2 ‘and 3 as related to the axle in Fig. 1. 8.5.3 Spurious Ultrasonic Indications from Contour Vari- cations—Because an axle varies in cross section it is possible to produce spurious indications, particularly at changes of ‘cross section. These must be recognized, and are not reason for rejection. It is not practical to define these indications in the specification, but the competent operator or technician will recognize these spurious indications as responses from axle contours. 8.5.6 Near-Field Resolution—It should be recognized that detection of discontinuities near the test surface is limited by the ultrasonic test frequency. In the case of heat-treated axles, this is approximately I in. (25.4 mm) from the test surface. 9, Retest 9.1 Ifthe results of the mechanical tests of any lot do not ‘conform to the requirements specified because a flaw devel- ‘oped jin the test specimen during testing, a retest shall be allowed if the defect is not caused by ruptures, cracks, or flakes in the steel, 9.2 Ifthe results of the mechanical tests of any lot do not conform to the requirements specified, the axles may be retreated, but not more than three additional times, end retests shall be made in accordance with Section 7. 10. Dimensional Tolerances 10.1. Length and Diameter: 10.1.1 For plain-bearing axles, the overall length shall not be less than the specified minimum length nor more than '& in, 3.2 mm) over. 10.1.2 For passenger-car roller-bearing axles ordered to finished length, the overall length shall not be less than the specified minimum length nor more than Yie in, (1.6 mm) over, 10.1.3 For all anles ordered for finished-end facing by the purchaser the overall length shall range from ‘a in. 0 4 in, (6.4 mm) over the specified minimum length, 10.1.4 For fteight-car rolle-bearing axles ordered to final length, the overall length shall not vary more than Ye in. (1.6 mm) over or under the specified length. 10.1.5 For any other axles ordered to final length and not ‘covered by the above classifications the overall length shall not be ess than the specified minimum length nor more than ‘ain. (3.2 mm) over. 10.1.6 The specified minimum length shall be the nom- inal overal final length less any allowable tolerances. 10.1.7 Rough-machined journals and wheel seats shall be ‘wto Ys in, (3.2 to 6.4 mm) over the finished diameters and Ys to "% in, of metal shall be allowed longitudinally at cach ‘change of cross section for finish machining. 10.1.8 The smooth-machined body shall be to the speci- fied size with no more than "4 in. (3.2 mm) over on the ah azt — gates FIG, 1. Showing Location of Referonce Holes in Axle tm) me yen one a by Ra Gm 8 esi ft: FIG. 2. Typical Distance-Amplitude Curve for a Heat-Treated Axle (88 Determined with a Sperry Rellectoscope, Type UM Using 2 1¥e-in. (28.5-mm) Diameter 2.25-MHz Quartz Transducer) diameters and shall have no more than % in. allowance Jongitudinally at each change of cross section, 11. Workmanship, Finish, and Appearance 111 The axles shall conform to the size and shape ified by the purchaser. Centering shall be a standard 60° with clearance drilled for lathe center points. 11.2 Axles shall be machined (o a smooth-machined finish between whee! seats. The wheel seats and journals shall bbe rough machined. The rough machining shall be free from objectionable ridges and chatter marks. 11.3 Fisish—The axles shall be free of injurious iraperfec- tions. The machining shall be done in a workmanship ‘manner to the contour specified 11.4 The interpretation of injurious imperfections in axles shall comply with Annex AI to this specification. 12, Inspection 412.1 Inspection of the axles shalt be made as agreed upon by the purchaser and seller as part of the purchase contract 12.2 The manufacturer shall afford the purchaser's in- spector all reasonable facilities necessary to satisfy him that the material is being produced and furnished in accordance ‘with this specification. Mill inspection by the purchaser shall not interfere unnecessarily with the manufacturer's opera- tions. All tests and inspections shall be made at the place of manufacture, unless otherwise agreed to. 13. Rejection and Rehearis 13.1 Any axle that fails to meet the requirements of this, specification shall be rejected. 13.2 Axles that show injurious imperfections subsequent to acceptance at the manufacturer's works will be rejected and the manufacturer shall be notified, 13.3. Samples tested in accordance with this specification that represent rejected material shall be preserved for 14 days from the date of the test report. In case of dissatisfaction with the results of the test, the manufacturer may request a rehearing within that time. Certification 14.1 Upon request of the purchaser in the contract or order, a manufacturer's certification that the material was manufactured and tested in accordance with this specifica- tion together with a report of the test results shall be furnished at the time of shipment, ss sce tin, (stam) csi oo) aes FIG. 3 Typical Diatance-Amptitude Curve for an Untreated Axle (es Determined with a Sperry Reflectoscope, Type UM Using a 1%, (21.5-mm) Diameter 1.00-MHz Quartz Transducer) PLAIN BRS. nore « nore 3 ro co wet U ROLLER BRS. nore s Nove 1—tabaratry Acceptance Samp: For use by purchase: to i ny accaptanen of sac 0 mare pr to Signe Od Nore 2 Sera number Nove 3-Manuactre’s naa or brand 9D. Starcard Stal Gummer. Pa JAW Stancrd Forged Products, ohnstown, Pa WMAP skews Poche Forgings. Moxens Rocks, Pe BOAP Oneprovky on & See Urabe HM Hora ta, vce, Poland TA Yrerton Works Lavin ie, Warton, Nove Seota CB Cotasma,Osasco, Brant NAW Motor, Cocapar, rant ST Fen Ancon, Rattan, England GF ASFOR Gunkerve. France Vi ASFOR, Valenones, Farce SMI Sarina, Osaka, Jape Sw SWASAP. Gomesion 5. Afton nore 2 nove pres nore ‘ Pres vores CIRCUMFERENTIAL DEVELOPMENT OF AXLE END Tomi Lovee tay ROR JngeeNerreo Tatuan, Crna Nore 4—Merit anc you made Nore 5G ot axe: ‘Geunvented double romalzed and tempers (G-—quenched and tompered H—tormalzed,qunched, and tompored Nove $-—Heat number, (GENERAL NOTES Al rears wi bo eps egy striped win tart notes a, righ and hse for eg ca ler beng axes ete’ axacer to berphery ot ba catenng nla, arufactere must Nash ens ero ae or Samping Al dovtore of sropuartes should be fed or ground ater Stanping The sbove are Uw rareram merkng requrements but te Iceatons on matical Kee may vay Wom Pat Mubvatd. FIG. 4 Standard Axle Marking 15. Marking 15,1 Axles shall be legibly cold stamped with steel stamps with letters and figures not less than Ye in, (6.4 mm) high in accordance with the requirements shown in Fig. 4. 15.2 In addition to the markings required in 15.1 and Fig 4, bar code tags may be applied to the axles. If these tags are applied, it is recommended that bar code 39 be used. The size and location of the tags, as well as the information to be included, shall be agreed upon by the purchaser and manu- facturer 16. USS, Government Procurement 16.1 When specified in the contract or purchase order, ‘material shall be preserved, packaged, and packed in accord- ance with the requirements of MIL-STD-163. The applicable levels shall be as specified in the contract or order. Marking for shipment of such material shall be in accordance with Fed. Std. No, 123 for civil agencies and MIL-STD-129 for military agencies. 17. Keywords 17.1 axles; rail applications ah a2t SUPPLEMENTARY REQUIREMENT ‘The following supplementary requirement shall apply only when specified by the purchaser. Details shall bbe agreed upon by the manufseturer and the purchaser, SI. Macroscopical Tests, SI.1 The prolongation from the largest axle in each hea shall be sawed normal to the axis of the axle and shall then be split longitudinally. The transverse and the longitudinal face shall be etched for macroscopical examination. Refer- ‘ence shall be made to Method E 381. ANNEX (Mandatory Information) Al. INTERPRETATION OF IMPERFECTIONS CONSIDERED INJURIOUS IN AXLES ALL General AL.L1 The conditions that have been. most difficult for inspectors to evaluate are light lines visible to the normal unaided eye, variously described as actual seams, hairines, stringers, shadow seams, ghost lines, etc, which appear after the axles have been finish machined’ and burnished or round. tis, therefore, advisable to describe these conditions in more detail. ‘AL.L2 The interpretation of injurious imperfections as enumerated below is not to be considered as precluding other unforeseen or objectionable conditions not specifically listed. The right of the purchaser is reserved to reject temporarily such axles and make final setlement on the basis of further negotiations between representatives of the manufacturer and the purchaser who are especially qualified to decide such questions ‘AL.L.3 Any transverse or circumferential seams, cracks, or laps of indeterminate depth on the axle surfaces other than the diseolorations listed in Al.I.4 regardless of their location, are considered to be injurious and are cause for rejection without further machining. AL.L.4 Ghost lines, shadow marks, or other similar disco! rations, visible to the normal unaided eye that are not actual separations in the metal are not considered injurious regardless of location. ‘ALLS Any longitudinal discontinuity, variously termed hailing, stringer, or fine seam, in machined filets is consid- ‘red to be injurious and is cause for rejection without further conditioning. AL2 Journals and Dust Guards Al21 Plain-Bearing Axles—Fine longitudinal discon- tinuities on the finished machined surfaces, variously termed haairlines, stringers, or fine seams, are not considered inju- rious if they meet the following conditions: AL2.1.1 Must not extend into fillets and must not have sharp edges. Journals must never be cleaned with a coarse abrasive or polished with emery under heavy pressure. Streaks, soratches, and some taper may result. The abrasive ‘may become embedded in the stee! and contribute to a “hot box.” Polishing may be done with artificial abrasive cloth (No. 180 grit or finer, free from ridges, selvage, etc.) using plenty of oil on a wooden block hollowed out to fit the journal, AL2.1.2 Must not be over “in. (12.7 mm) long individ ually. AL2.1.3 Total length of such imperfections, Va in. (6.4 mm) to Ye in, (12.7 mm) long, must not exceed 1¥2 in. (38.1 ‘mm) in any one end of the axle. AL2.1.4 Within any 3ein. (76.2-mm) length there may not be more than two such imperfections, Yin. (6.4 mm) to Ye in. (12.7 mm) long, i line with each other in any one end of axie. AL.22 Roller-Bearing Axles—Fine longitudinal discon- tinuities on the finished (burnished or ground) surfaces variously termed hairline, stringers, or fine seams are not considered injurious if they mect the following conditions: AL22.1 Must not extend into fillets. 1.2.2.2 Must not be over ¥%4 in. (19.1 rm) long individ- ually in the journal nor ¥ in. (12.7 mm) long individually in the dustguard seat. A1.2.2.3 Total length of such imperfections over Ye in, (64 mm) long must not exceed 2 in. (50.8 mm) in any one end of axle AL2.3 Refiishing—Burnished plain journals showing imperfections in excess ofthe limitations outlined in Al.2.1 may be reconditioned by refinishing 10 2 diameter not smaller than 0.020 in, (0.5 mm) under the nominal diameter, If, after refinishing the axles mect the requirements of Al.2.1 above they may be considered acceptable. AL. Wheel and Gear Seats AL3.1 Freight Car Axles (Plain and Roller Bearing)— Longitudinal seams in wheel seats of freight car axles are not considered injurious i they meet the following conditions: ‘AL3.1.1 Must not extend into the dust guard or body filets ‘AL3.1.2 Must not be over 2 in. (50.8 mm) long individ- ually. ‘AL3.1.3 Total length of such imperfections, Ye in. (6.4 mm) to 2 in, ($0.8 mm) long, must not exceed 4 in. (102 mm) in any one end of axle. ALA All Other Axles ‘A141 Longitudinal discontinuities on the finished-ma- fh azt chined surface of wheel and gear seats, variously termed hairlines, stringers, fine seams, tight seams, surface imperfec- tions, etc, are not considered injurious if they meet the following conditions: AL4.11 Must not extend within 1% in, (38.1 mm) of either end of wheel or gear scat ‘Al.4.1.2 Must not be over ' in. (12.7 mm) long individ- wally. ‘AL.4.1.3 Total length of such imperfections, 4 in. (6.4 mm) t0 12 in, (12.7 mm) long, must not exceed 3 in. (76.2 mm) in any one end of axle ALS Areas Between Wheel (and Gear) Seats (Body) ALS.1 Machined Bodies—Longitudinal discontinuities oon the finished surfaces, variously termed airlines, stringers, or fine seams, are not Considered injurious if they mect the following conditions: ALS.) Must not extend into fillets adjacent to wheel or ear seat ‘AL5.2 Must not be over ¥ in, (12.7 mm) long individu- ally. AL.S.3. Total length of such imperfections, in. (6.4 mm) to Yin, (12.7 mm) long, must not exceed 1 in, (38.1 mm) in any 12 in, (305 mrn) of body length ALS4 Axles containing longitudinal discontinuities inthe body in excess of those described in AI.S.2 and AL.5.3 above may be reconditioned by grinding or machining provided the diameter is not reduced below the specified limit. ‘Tne American Soil fr Testing and Matra tates ne postion espacting he vay of ay patent ges assed in corracton ‘wah any tr enone vs Sander. Users of his stancrd are eres aie tat determination ofthe vay of ey such atom nga, nd pe neko itingomert of such igh, rear fe ew response This standard ebjoctorvton at any tre by te responsi tecnica commie and munt ba eviewod every te yours and notreced, etna rapproves wih You Comer ar tad ath fr rion of ie sardudor redone anda ‘nd shod be adrersed 0 ASTA Headgutor.Yourconmarts wil cob cared caraeatn ata masing ofa rexponaie technica! commas whch you rey exon I You lata! your comments have At reeled a Pearing you shou make Yor ‘rows inci fhe ASTM Commrtee on Standercs, 1918 Race St, Pingea, PA 75103.

You might also like