Long-Life Asphalt Pavements - Technical2007
Long-Life Asphalt Pavements - Technical2007
Long-Life Asphalt Pavements - Technical2007
1
Long-Life Asphalt Pavements
Technical version
Long-Life Asphalt Pavements Technical version June 2007
2
European Asphalt Pavement Association
Rue du Commerce 77
1040 Brussels,
Belgium
www.eapa.org
info@eapa.org
July 2007
Long-Life Asphalt Pavements Technical version June 2007
3
Content page
1. Introduction 4
1.1. Background 4
1.2. Definition of long-life pavements 5
2. Construction of new pavements 6
2.1. The pavement structure 6
2.1.1. Surface course 7
2.1.2. Binder course 8
2.1.3. Base course 8
2.1.4. Unbound materials and foundation 8
2.2. Design 8
2.2.1. Fatigue cracking 10
2.2.2. Permanent deformation 11
2.2.3. Other mechanisms 11
2.2.4. Improved design methods 11
2.3. Construction 12
2.4. Maintenance 13
3. Economic aspects 13
4. Future developments 14
4.1. Procurement and specifications 14
4.2. Improved economic models 14
5. Summary and conclusions 15
6. Literature 16
Appendix: Durability of surface layers in Europe 18
A.1. Introduction 18
A.2. Asphalt mixtures 18
A.3. Basic assumptions for determining the durability of the surface layers 20
A.4. Results 21
Long-Life Asphalt Pavements Technical version June 2007
4
1. Introduction
An important goal in the pavement industry is to provide constructions at ever lower
life-cycle costs, a goal requiring continuous development in areas such as design,
material characterization and production, as well as maintenance techniques and
management. During the last couple of years, the concept of Long-life pavements
1
(LLP) has been established in Europe and America. The main purpose of this concept
is to develop a framework, in which more cost-effective pavements are produced. The
LLP-concept is to some extent based on earlier concepts, such as full-depth, stage-by-
stage and deep-strength designs, but mainly on more recent advances in material
technology, design and functionality. In practice, the intention of the LLP-concept is
to significantly extend current pavement design life by restricting distress, such as
cracking and rutting, to the pavement surface. Common distress mechanisms such as
bottom-up fatigue cracking, rutting in the unbound layers and frost heave should, in
principle, be completely eliminated.
When the availability of road lanes and the road user delay costs are taken into account
in the cost-benefit analyses of pavements it will show that a number of highways in
densely populated areas require low maintenance pavements. That means a total
reconstruction of a road pavement is hardly possible or even impossible.
This is one of the reasons for developing the Long-Life Pavement concept.
The purpose of this paper is to provide a state-of-the-art review of developments in
long-life asphalt pavements.
1.1 Background
All elements of long-life pavements are not by any means new and some have been
circulating in different forms for a considerable time. For example, several countries
have utilised so-called full-depth asphalt pavements consisting of relatively thick
bitumen-bound layers directly constructed on the sub-grade or placed on relatively
thin granular base courses. One of the main arguments for this type of design is that
the overall pavement thickness can be kept relatively thin compared to conventional
designs consisting of relatively thin bitumen-bound layers on relatively thick granular
layers. In addition to this obvious advantage, during the years it has been recognized
that full-depth and deep-strength pavements often have shown design lives
significantly longer than initially expected [1.]. Similar experiences to those
mentioned have been recognised in the UK, where investigations on motorways
suggest that fatigue cracking and structural deformation are not prevalent in pavements
which are constructed with sufficient strength (above a certain level). The main
conclusions suggest that well-constructed flexible pavements show very long service
lives provided that distress mechanisms such as rutting and cracking are confined to
the pavement surface, which significantly facilitates maintenance [2. and 3.].
During 1998/1999, the Conference of European Directors of Roads (CEDR) declared,
as suggested by the UK Highways Agency, that so-called Long-Life Pavements were
an appropriate area for co-operative research. Subsequently, a working group called
1
It should be emphasised that the term long-life pavements given in this paper is a collective name incorporating
many of the features shared by concepts such as perpetual, long-lasting, heavy duty and maintenance free
pavements.
Long-Life Asphalt Pavements Technical version June 2007
5
ELLPAG (European Long-Life Pavement Group) was established as a focal group for
determining the way forward. The objectives of ELLPAG include producing state-of-
the-art reports on European knowledge on the design and maintenance of long-life
pavements. In the long run, a user-friendly comprehensive Best Practice guidance
document for all types of pavements is intended to be produced [4.].
In the USA, the concept termed Perpetual pavements has rapidly gained acceptance
following workshops on the concept held in the first years of the new millennium. One
of the publications arising from these is a synthesis published by the Asphalt
Pavement Alliance (APA), a coalition of the National Asphalt Pavement Association
(NAPA), the Asphalt Institute (AI) and the State Asphalt Pavement Associations
(SAPA) [5.]. Relevant material presented at the Transportation Research Board (TRB)
Annual Meeting in 2001 was published in Transportation Research Circular 503
Perpetual Bituminous Pavements [6.]. This long-life approach aims at extending the
20-year life expectancies of hot-mix asphalt pavements to greater than 50 years [6.].
The term Perpetual Pavements is to some extent a rewriting of long-life pavements,
but focuses on resisting specific distresses in the each bound layer. In this case, the
surface course, binder course and base courses are selected, designed and performance
tested in accordance with deterioration mechanisms such as permanent deformation
and fatigue cracking. In addition to long-life and perpetual pavements, several other
approaches have been used, each comprising different parameters and techniques.
As indicated in this section, the long-life concept is not a single coordinated drive
towards improved pavements. The common feature among different approaches within
the long-life pavement concept described here is the objective to gather knowledge
regarding design, material characterization and production, as well as maintenance
techniques and management methods to produce pavements with long life in order to
achieve low life-cycle costs. Consequently, even though the long-life concept may
appear homogenous, many significant differences arise between different
organisations and researchers regarding design, material selection and production
methods. In addition to the two approaches mentioned (long-life pavements and
Perpetual Pavements, respectively), some countries, including France, Germany, USA
and the UK, already permit design periods in excess of the frequently used 20 years
[4.]. However, it should be emphasised that in Europe, solely the UK states that their
pavements are designed for 40 years [4.]. In countries such as the Netherlands, flexible
pavements of motorways are designed in such a way that structural damage will be
avoided. In the past they used the Stage-by-stage concept; the existing pavement
was overlaid to become a long-life-pavement. Now the structural design is based on
long life taking into account expected functional use of the road. In the Netherlands
the traffic intensities are very high and therefore the disruption to traffic has to be
avoided. The availability of the road is of utmost importance. The repair of structural
damage is too costly and too time consuming. In other countries, e.g. France,
pavement design life is guided by an economic strategy, which usually is carried out
over 30 years. Since most countries possess national pavement design methods, based
on local materials and local experience, only a general strategy for long-life pavement
design and construction will be described in this document.
1.2 Definition
In the literature several definitions of long-life pavements have been given. In the
USA, perpetual pavements has been closely connected to thick asphalt pavements
comprising a three-layered asphalt pavement including a wear-resistant and renewable
Long-Life Asphalt Pavements Technical version June 2007
6
top layer, a rut-resistant and durable intermediate layer and a fatigue-resistant and
durable base layer [6.]. This concept represents an operational definition, or example
of a long-life pavement, but it restricts long-life pavements to a certain design. The
synthesis presented by the Asphalt Pavement Alliance (APA) defined a perpetual
pavement as an asphalt pavement designed and build to last longer than 50 years [5.].
ELLPAG [4.] uses a similar functional definition:
A long-life pavement is a type of pavement where no significant
deterioration will develop in the foundations or the road base layers
provided that correct surface maintenance is carried out.
The ELLPAG definition above came from the intention to avoid limiting the concept
to a specific life (e.g. 30, 40 or 50 years), which has done in some studies (e.g. [7., 3.
and 1.]). In this paper, the functional definition of ELLPAG has been adopted, which
consequently implies that all pavement layers, except the surfacing, are considered as
permanent. To maintain the overall objective, it is necessary to successively monitor
pavement performance in order to ensure that all distress mechanisms are limited to
the surface layer.
Figure 1 illustrates how the goals of the LLP-concept can be approached. The figure
illustrates important quantitative components which have been identified by researchers
to achieve long-life performance. In addition to the guiding components, some
requisites are important to consider when designing a LLP. Pavement network funding
normally comes from the government by budget allocations and effective network
management requires that the budget levels are at least sufficient to keep the core road
assets in stable condition in the long term. In the case of LLP, the expected increased
construction costs associated with improved materials and construction constitute
financial restraints even though lower life-cycle costs are obtained in time (see Section
3). In addition, the final design of a LLP depends on local conditions such as sub-grade
type, present and future traffic volumes and materials available. From these so-called
prerequisites, the ultimate goal of low life-cycle costs can be obtained based on
optimizing maintenance activities, delay and environmental costs.
Figure 1. Prerequisites, components and goals of long-life pavements concepts
Prerequisites
Sufficient financing
Knowledge regarding
local conditions
- Subgrade types
- Traffic volumes
- Available materials
Components
Design
- Design life, e.g.>40 years
- Conservative design criteria
Performance specifications
- Wear-resistant top layer
- Rut-resistant layers
- Fatigue-resistent base course
Periodical resurfacings
Goals
Low life-cycle costs
- Few maintenance activities
- Low delay costs
- Low environmental costs
Long-Life Asphalt Pavements Technical version June 2007
7
2. Construction of new pavements
Today, most countries regard the public road transportation system as an essential pre-
condition for economic development and welfare. It is therefore important that the
asset is managed professionally through all stages including design, construction and
maintenance.
2.1 The pavement structure
A flexible pavement consists of the road structure above the formation level, which
normally comprises bitumen-bound and unbound materials. The pavement structure
should be able to resist the traffic and environment to which it will be exposed in such
a way that structural distress mechanisms are avoided. Normally, pavements are
designed as layered structures with relatively low strength in the lower layers and
materials with progressively increasing strengths towards the top (see Figure 2). The
rationales for this arrangement are both technical and economic.
Figure 2. Schematic illustration of flexible pavement structure.
In general, the asphalt layers are laid on a bound or unbound road base layer. Starting
at the road surface, the first layer is called the surface course. The second layer is the
binder course and the lower layers are the base courses.
For a good bearing capacity of the whole road structure it is important that there is a
good bond and interlock between all the (bituminous) bound pavement layers and a
good interlock between the unbound pavement layers. It of course also applies to the
interlock between the first asphalt layer and the unbound base beneath it.
For the durability of the asphalt structure, it is also essential to have a good bond
between the asphalt layers that can avoid water penetrating between asphalt layers.
2.1.1 Surface course
The surface course constitutes the top layer of the pavement and should be able to
withstand high traffic- and environment-induced stresses without exhibiting
unsatisfactory cracking and rutting in order to provide an even profile for the comfort
of the user and at the same time possessing a texture to ensure adequate skid
resistance. Depending on local conditions, functional characteristics such as skid
resistance, noise reduction and durability are often required for surface courses. In
some cases, rapid drainage of surface water is desired through a porous surface while
in other cases the surface course should be impermeable in order to keep water out of
the pavement structure. As indicated, the surface layer is important for the pavement
TERRASSYTA
UNDERGRUND
BRLAGER
BELGGNING
FRSTRKNINGSLAGER
TERRASSYTA TERRASSYTA
UNDERGRUND UNDERGRUND
BRLAGER
BELGGNING
FRSTRKNINGSLAGER
BRLAGER BRLAGER
BELGGNING BELGGNING
FRSTRKNINGSLAGER FRSTRKNINGSLAGER
Asphalt layers
Unbound road-base
Formation
Subgrade
Unbound sub-base
Long-Life Asphalt Pavements Technical version June 2007
8
performance but no single material can provide all the desired characteristics (e.g.
porous and impermeable at the same time). A wide range of surface layer products can
therefore be considered appropriate depending on specific requirements:
Asphalt Concrete (AC)
Bton Bitumineux Mince (Thin Layers Asphalt Concrete AC-TL)
Asphalt Concrete Very Thin Layers (AC-VTL)
Ultra Thin Layer Asphalt Concrete (UTLAC)
Stone Mastic Asphalt (SMA)
Hot Rolled Asphalt (HRA)
Porous Asphalt (PA)
Double layered Porous Asphalt (2L PA)
Mastic Asphalt (MA)
Soft Asphalt (SA)
In the end, the selection of the surface course is a matter of identifying the most
appropriate material during the design process. The functional requirements can
conflict. For example, noise reduction could require the use of a double-layered
porous asphalt and that conflicts with the requirement of a very durable surface layer.
The durability of surface layers can be improved by using higher quality materials.
The higher costs of these will be compensated by the lower costs of traffic measures
and user costs.
In Appendix A the durability of these surface layers is shown.
2.1.2 Binder course
Under the assumption that a particular layer solely is subjected to a mode of
deterioration, long-life pavements are usually designed by preventing permanent
deformation in the bound layers using an appropriate binder course. Binder courses are
frequently adopted on the assumption that the highest shear stresses will occur about
50 70 mm below the asphalt surface. The binder course is therefore placed between
surface course and base courses to reduce rutting by combining qualities of stability
and durability. Stability can be achieved by sufficient stone-on-stone contact,
combined with stiff and/or modified binders.
2.1.3 Base course
The base course is perhaps the most important structural layer of the pavement, which
is intended to effectively distribute traffic and environmental loading in such a way
that underlying unbound layers are not exposed to excessive stresses and strains. This
often implies comparatively high stiffness of the base course. However, following the
principle of performance-specific design of each layer, the base course should
primarily show adequate fatigue resistance. Consequently, it is often assumed that for
an asphalt mixture, there exists incompatibility between stiffness and fatigue-
resistance. This assumption is based on the fact that a stiff base course can be obtained
using either relatively course aggregate or stiff bitumen, which both increase the
sensitivity to high strain levels [8.]. In principle, a base course material is affected by
all material-related factors including grading, additives as well as air void and binder
contents. In practice, relatively fine grading [9.], low void content [10.] and high
binder contents are strived for. According to APA [5.], there are several possible
strategies to achieve a base course exhibiting long-life characteristics. One approach to
ensure good fatigue life, as determined by a given laboratory test and a given
Long-Life Asphalt Pavements Technical version June 2007
9
pavement construction, is to restrict the tensile strain at the bottom of the base course
below a certain fatigue limit, under which no damage develops. However, the
identification of such a limit is in practice very difficult.
2.1.4 Unbound materials and foundation
Since the formation and sub-soil often constitute relatively weak materials, it is of
utmost importance that the applied loadings are effectively eliminated by the layers
above. Especially, high vertical strains may require relatively thick layers. In this case,
unbound road-base or sub-base layers consisting of uncrushed aggregate or crushed
aggregate can be suitable. Generally, unbound materials originate from locally
available sources, such as native soil, crushed/uncrushed granular materials and re-
used (secondary) material. The type and thickness of the unbound materials used for
the unbound road base layers technically depend on the structure to be designed
(traffic loading) and the stiffness of the sub-grade. In some countries, climatic
conditions may also require relatively thick pavement structures in order to avoid
frost-related heaves. Furthermore, economic factors, such as availability and
transportation costs, also have a significant impact on the amount of unbound
materials desired in a pavement. In some cases adequate bearing capacity can be
achieved using different stabilization techniques. For example, different types of
cement- or lime-stabilization can be used to improve clays.
2.2 Design
Today, pavement design is normally represented by so-called semi-mechanistic
methods, implying that they partly are based on fundamental engineering principles.
Semi-mechanistic procedures consist in principle of a structural response model and
associated performance models (see Figure 3). Response models relate traffic loading
to stresses and strains in the pavement structure, while performance models relate
calculated stresses and strains to rate of deterioration. As indicated in Figure 1, the
actual design life is an essential feature of the LLP-concept. In most European
countries, a design life of 20 years is adopted. Only in the UK is it explicitly stated
that pavements should be designed for 40 years when economically viable [4.].
Even though a number of potential deterioration mechanisms exist, the two main
distresses considered in semi-mechanistic methods are rutting, originating in the sub-
grade, and fatigue cracking, initiated in the bottom of the asphalt layer. Structural
rutting originating at the sub-grade is considered by limiting the compressive strain
induced at the top of the sub-grade, normally as a function of the expected number of
load applications during the design period and the thickness and stiffness of the
pavement layers. These two traditional design criteria were originally based on
laboratory testing and field performance of pavements whose layers were relatively
thinner than pavements designed for current relatively high traffic levels.
According to a recent European investigation [11.], the importance of traditional
fatigue cracking and rutting in the sub-grade is nowadays questionable. In this
investigation, fatigue cracking and rutting in the sub-grade were only considered to be
ranked as numbers 6 and 9, respectively. Other deterioration mechanisms such as
rutting in the bituminous layers and surface-initiated cracking were considered far
more important: ranked as number 1 and 2, respectively. However, even though
distress mechanisms associated with cold climate such as frost heave, wear due to
studded tyres and low-temperature cracking, achieved low ranking (number 10, 11 and
12, respectively), they may be significant in some countries such as Sweden.
Long-Life Asphalt Pavements Technical version June 2007
10
In contrast to traditional fatigue cracking and rutting in the sub-grade, the other
deterioration mechanisms (such as rutting in the bituminous layers, crack initiation in
the surface layer), are difficult to address in (the old) semi-mechanistic design
methods. One way of including these mechanisms is therefore to prescribe functional
demands using different simulation methods (functional laboratory tests).
Figure 3. Schematic illustration of semi-mechanistic design method.
Figure 4. Example of pavement structure and the two traditional design criteria.
In general, deterioration, such as fatigue, is within the semi-mechanistic framework
generally obtained from laboratory testing, which is assumed to represent field
Traffic loading Climate Pavement structure
Material properties
Response model
,
Performance model
Fatigue Deformations ?
Base courses
Binder course
Surface course
(Un)bound roadbase
Tensile strains
Subgrade
Compressive strains
Bound
materials
Unbound
materials
Long-Life Asphalt Pavements Technical version June 2007
11
conditions. Fatigue testing is usually performed by applying a cyclic loading (strain-
or stress-controlled), often at a given test temperature and frequency, to an asphalt
mixture specimen. The fatigue results obtained at laboratory testing are subsequently
related to the strain response obtained from the structural model. Consequently, the
life of a given pavement structure subjected to repetitive traffic loading can be
calculated when the strains in the structure as well as the relationship between the
strains and deteriorations have been established.
2.2.1 Fatigue cracking
Fatigue is one of the main distress mechanisms considered in flexible pavement design
and is generally considered to be caused by excessive tensile strains due to repetitive
traffic loading. The loading results in growth and coalescence of pre-existing or
initiated microscopic defects, which finally cause the asphalt layer to crack.
Eventually, the entire bearing capacity of the pavement structure may be jeopardized.
An increased asphalt thickness reduces the traffic-induced strains in the bottom of the
bituminous base layer and, consequently, increases the fatigue life.
In principle, the design philosophy of long-life pavements does not differ significantly
from traditional semi-mechanistic design methods. However, due to the aim of
restricting structural deterioration to the pavement surface, conservative design criteria
should be employed. In the UK, the design traffic for 40 years is determined in a
similar manner to that of a 20 year life with enlarged traffic multiplier to account for
the greater growth in traffic over the extended period. Pavements design above a
traffic level of 80 million standard axles (80 kN) are said to be designed as long-life
pavements [4.]. The rationale for this traffic level is supported by empirical and
analytical studies [2. and 4.].
In order to eliminate structural deterioration, some investigations have suggested that
conventional transfer functions (i.e. performance models, cf. Figure 3) should be
replaced by explicitly expressed conservative thresholds for allowable strain values.
For example, Monismith and Long [12.] suggested that the maximum tensile strain at
the bottom of the asphalt layer should be restricted to 6010
-6
. It should be
emphasised that the threshold level given by Monismith and Long may not be
universally applicable since they are derived using a given pavement system, design
method, bituminous mix and laboratory test equipment. However, in principle it
should be possible to derive corresponding threshold values for other pavement
configurations and values in the range of 50-7010
-6
m/m have been reported as
fatigue thresholds [13., 14. and 15.]. For the sake of convenience, it should be
emphasised that any design parameter and criterion given should not be taken out of
context since they are closely linked to a specific design guide and testing method
used.
2.2.2 Permanent deformation
The other major deterioration mechanism considered in semi-mechanistic design is
rutting, originating in the sub-grade. As in the case of fatigue cracking (see Section
2.2.1), most semi-mechanistic methods are equipped with performance models for
calculating permanent deformations using transfer functions.
In order to eliminate structural deterioration, some investigations have suggested that
conventional transfer functions (i.e. performance models, see Figure 3) should be
replaced by explicitly expressed conservative thresholds for allowable strain values.
Long-Life Asphalt Pavements Technical version June 2007
12
For example, Monismith and Long suggested that the maximum vertical compressive
strain at the top of the sub-grade should be restricted to 20010
-6
m/m.
2.2.3 Other mechanisms
Traditionally, fatigue cracking has been viewed as initiated in the bottom of the
asphalt layer to propagate up through the layer (bottom-up cracking). However, there
are other forms of fatigue-related cracking than traditional bottom-up cracking, such as
reflective cracking. The latter deterioration mechanism is caused by repetitive
shearing, e.g. when a new asphalt layer is laid upon an already cracked layer. With
time, the crack will propagate through the new layer. A third type of fatigue is surface
initiated (top-down) cracking. This type of fatigue cracking is considered to be caused
by a complex combination of pavement structure, load spectra and material
characteristics. Even though still disputed, this deterioration mechanism motivates a
certain fatigue-resistance of the surfacing. In addition to fatigue cracking and rutting,
some semi-mechanistic methods also take low-temperature cracking and frost heave
into account. Another deterioration mechanism which should be accounted for is
ageing. This distress mainly affects the bituminous layers and is manifested by
increased stiffness and decreased flexibility. According to Nunn et al [2.] a road is
more susceptible in its early life before the structural properties have been increased
by curing. In this case, curing implies increased bearing capacity due to gradual
increase in asphalt stiffness. However, whether or not increased stiffness is desirable
depends on whether, or not, the stiffening extends pavement life and lowers overall
life-cycle cost. In certain cases, it is not unlikely that ageing will result in low
temperature cracking but also complicates recycling. Consequently, it will in many
cases be desirable to minimize ageing by reducing the air void content of the mixture.
A common denominator of the distress mechanisms mentioned in this section is that
they are difficult to take into account using semi-analytical methods. Some of the
distresses are considered to require more advanced response and/or performance
models (see Figure 3). In the case of top-down cracking and permanent deformations
in the bitumen-bound layers, new and improved design methods may take this into
account in the future.
However, functional demands may be used to take these mechanisms into account. For
example, the adequacy of a binder course can be evaluated using a simulation method.
If a material shows superior resistance against a certain distress mechanism simulated
by the test it may be judged appropriate to be used in the design.
2.2.4 Improved design methods
Today, there are several design methods available for pavement design.
At the National Center for Asphalt Technology (NCAT) at Auburn University in
conjunction with the Asphalt Pavement Alliance (APA) a procedure was developed
for the mechanistic-based design of flexible long-life or perpetual pavement structures.
This is a program called PerRoad. [19.]
The design software utilizes layered elastic theory to compute critical pavement
responses under axle load spectra. Monte Carlo simulation is used to model the
uncertainty corresponding to material, loading and construction variability. The
program can be used as a design and analysis tool to assess the likelihood that critical
pavement responses will exceed a threshold set by the analyst. Additionally, transfer
Long-Life Asphalt Pavements Technical version June 2007
13
functions may be used to determine a damage accumulation rate for pavement
responses exceeding the threshold.
This software uses U.S. customary units, commonly known in the United States as
English units.
2.3 Construction
Like traditional pavement construction, the construction of LLP should at least be
executed in accordance with public requirements. In this case, technical and functional
requirements on LLP should in general be higher compared to traditional pavements.
One way of ensuring higher quality is to prescribe functional demands instead of
technical specifications. This emphasises the contractors roll in achieving long-life
performance compared to when technical specifications are used. When functional
demands are used, it is up to the contractor to show that a solution meets the
requirements. At least two benefits can be identified:- improved flexibility, meaning
that several solutions may be considered, and an increased concern from the contractor
to optimize the production, e.g. compaction.
The transportation of the asphalt mixture from the asphalt plant to the construction site
is important for the durability of the pavement. During transport the temperature of the
asphalt mixture should not drop too much and one should be aware of possible
segregation. During transportation there could occur temperature segregation and/or
mixture segregation. Material Transfer Vehicles that remix the mixture could be used
to avoid temperature and mixture segregation. Adequate quality control during
construction is essential too. In this way all the relevant issues will be monitored.
One of the most important construction-related aspects is mixture composition. An
optimal recipe should result in a homogenous material structure which facilitates
adequate compaction. Results presented in [7, 21] indicate that 3 percent more
compaction results in 15 percent less thickness needed due to improved fatigue
behaviour (in this case 8% air voids versus 5% air voids). Low void and high binder
contents will also improve fatigue characteristics as well as enhance resistance against
moisture-related damage, which is important since the base course layer often is in
prolonged contact with water. Perhaps the most advocated material-related
improvement is to modify the bitumen using different polymers. Many studies have
indicated that polymer modified bitumen produces pronounced improved fatigue
behaviour of a given mixture type (e.g. [16.]). The combination of a thick well-
constructed pavement and a fatigue-resistant base course is considered sufficient to
guard against traditional fatigue cracking.
In the context of long-life pavements, it is still necessary to periodically replace the
surface course in order to fulfil the aim of avoiding structural deterioration. In the UK,
two quite different routes have occurred [2.]. In order to improve durability, thicker
asphalt layers have been introduced in order to achieve improved compaction. On the
other hand, UK has experienced an increased interest in the use of relatively thin hot-
mix surface courses (Thin Layers of Asphalt Concrete). Investigations on motorways
in the UK have suggested that fatigue and structural deformation do not occur in
pavements which have been constructed with sufficient strength to resist structural
deterioration. The main conclusions suggest that well-constructed flexible pavements
show very long service life provided that distress mechanisms such as rutting and
cracking are confined to the pavement surface [2. and 3.].Asphalt mixtures are
viscoelastic composite materials which show significant time- and temperature-
Long-Life Asphalt Pavements Technical version June 2007
14
dependence. At high temperatures and/or low loading rates (vehicle speed), asphalt
mixtures are relatively soft, while the opposite applies at low temperatures and/or high
loading rates. Another characteristic of asphalt mixtures is the gradual stiffening with
time, ageing. The adequacy of asphalt mixtures in flexible pavement design depends
on the quality and composition of the main constituents: bitumen and aggregates.
Binder properties, such as stiffness and ductility, have a well-documented effect on
mixture performance since the stiffness of the binder largely influences the stiffness of
the mixture. The bituminous binder should be chosen taking into consideration the
prevailing conditions concerning aggregate type and regional climate since they
collectively influence mixture performance. In some respects, asphalt binder and
mixture properties can be improved using certain additives, e.g. polymers. In addition
to binder properties, binder content shows a major impact on mechanical properties of
asphalt mixtures. The aggregate should exhibit adequate properties regarding mainly
stability and wear resistance.
2.4 Maintenance
In the past, the preoccupation of road engineers has been mostly with construction of
new roads. However, as road networks in many countries have been completed, the
emphasis has gradually turned to maintenance of the existing network [17.]. In
contrast to relatively short-duration construction projects, maintenance is characterised
as an on-going long-term process over a relatively widespread area.
Maintenance of traditional roads normally covers a wide range of activities aimed at
reducing the rate of pavement deterioration and in the end achieve low vehicle-
operating costs. As more advanced maintenance activities, such as reconstruction, are
significantly more expensive than resurfacing, it is important to continuously carry out
adequate activities in order to avoid an increased deterioration rate. A third reason for
carrying out maintenance is to keep the road open continuously. Any failure to keep a
highly trafficked road open will lead to serious social and economic consequences.
For this reason structural damage has to be avoided; repairing structural damage is
costly and time consuming. In contrast to traditional pavements, long-life pavements
are defined as pavements, which do not show any structural deterioration.
Consequently, the end of a pavements life will not be reached as long as correct
surface maintenance is carried out.
For motorways with a very high traffic intensity the availability of the road is of
utmost importance and therefore disruption to traffic has to be avoided. The
maintenance or the renewing of the surface layer has to be done in a short time period
to minimise the hindrance to the traffic. Besides that the cost of traffic management
measures during maintenance works on motorways are high and can be more then
50% of the total job costs.
The lower need for more extensive structural maintenance activities with LLP
certainly affects the pavements overall life-cycle costs.
Long-Life Asphalt Pavements Technical version June 2007
15
3. Economical aspects
As discussed in Section 1, the overall purpose of LLP is to achieve lower annual costs
by increased pavement life and fewer and more cost effective maintenance activities.
In order to assess the economic benefits of LLP, the full financial consequences
should be considered using Cost/Benefit Analysis (CBA) [4.]:
Initial construction costs
The loss of pavement capital due to pavement deterioration
Agency costs due to periodic maintenance and traffic management at road
works
Road user costs, primarily due to delays at road works
The costs due to accidents involving road users and workers at road work
sites
The environmental economical impacts of road construction and
maintenance
Intuitively, a LLP probably results in an increase in construction cost compared to
traditional pavements, but lower maintenance-related costs. Some of the costs
included in CBA are relatively simple to determine while others are relatively
difficult. In the case of pavement deterioration, only limited information regarding
costs has been published. The most likely explanation is that present Pavement
Management Systems (PMS) mostly do not include residual value of pavements [4.].
Costs associated with road user delays can be obtained using models based on
measured traffic flows and road capacities. Road safety costs are more difficult to
appreciate, primarily due to lack of relevant data. The three main areas of concern for
environmental costs are recycling of pavement materials, pollutant impacts related to
fuel consumption and noise impacts related to maintenance work. The agency costs
consist mainly of direct costs including maintenance and traffic management costs but
also indirect costs in terms of administration. The review presented by FEHRL [4.]
showed that only the UK takes special account of the economic aspects of LLP. Using
CBA, UK experience has shown that pavements classified as LLP are expected to be
more cost-effective than traditional road pavements since the small increase in
construction cost is compensated by lower direct maintenance costs and indirect
disruption-related costs. For a 10 year period, the total savings by adopting the LLP
principal in the UK, are expected to reach 350 Million Euro [4.].
However, even though many costs associated with CBA are abstract and difficult to
establish, there are simpler ways of estimating the economic benefits of a LLP.
Perhaps the easiest way is to compare the construction and maintenance costs of two
(or more) types of pavement structures, one being a LLP and the other being a
conventional one. This in turn requires that the design models used are capable of
taking into account the different parameters responsible for the deterioration.
The traditional Life Cycle Cost Analyses (LCCA) can be used for calculating the
present worth of costs for pavement alternatives and it is the primary tool used for
economic comparisons.
For these LCCA studies the time span that is taken into account is mostly between 20
and 40 years. When dealing with Long Life Pavements this time span should be longer
and might have to go up to 100 years.
Long-Life Asphalt Pavements Technical version June 2007
16
In [20.] Haas et al. suggest a framework for LCCA applications which recognizes
short, medium and long term cycle periods, functional class of highway, public and
private sectors and likely or preferred LCCA method. Reasonable life cycle periods for
short, medium and long term analysis are in the order of 25, 50 and 100 years
respectively. This paper [20.] also gives a numerical example which shows how an
agency could calculate an internal rate of return (IRR) for a base investment
alternative involving a long life pavement design.
4. Future developments
4.1 Procurement and specifications
An important aspect, which affects the final result in the field, is the means by which
quality is defined, measured, controlled and ensured. In recent years, performance
specifications for pavements have been debated intensively. Performance
specifications are often considered to recognize the relationship between construction
quality and long-term performance. By rationally controlling variables that impact
long-term performance, the quality of the final product can be improved. In order to
achieve long-life performance, aspects such as these should be considered in addition
to the technical demands.
4.2 Improved economic models
As indicated in Section 3, improved economic models are necessary to show the
benefit of alternative designs and materials. Perhaps the most significant obstacle is
the need to develop a model which is capable of illustrating the relation between
investment cost and life-cycle costs. Today, most pavements are purchased primarily
based on investment cost, which consequently, often leads to high life-cycle costs
since the procurement procedure rewards the lowest bidding price.
5. Summary and conclusions
During the last couple of years Long-Life Pavements- and Perpetual Pavement
concepts have been established in Europe and in the USA. The main purpose of these
concepts is to develop a framework, in which more cost-effective pavements can be
produced.
When the availability of road lanes and the road user delay costs are taken into account
in the cost-benefit analyses of pavements it will show that a number of highways in
densely populated areas require low maintenance pavements. That means a total
reconstruction of a road pavement is hardly possible or even impossible.
This is one of the reasons for developing the Long-Life Pavement concept.
A long-life pavement is defined as a type of pavement where no significant
deterioration will develop in the foundations or the road base layers provided that
correct surface maintenance is carried out.
This definition implies that all pavement layers, except the road surface layer are
considered as permanent pavement layers.
Long-Life Asphalt Pavements Technical version June 2007
17
The LLP-concept is to some extents based on earlier concepts but mainly on recent
advances in material technology, design and functionality.
In practice, the intention of the LLP-concept is to significantly extend current
pavement design life by restricting distress, such as cracking and rutting to the
pavement surface. Common distress mechanisms such as bottom-up fatigue cracking,
rutting in the unbound layers and frost heave should, in principle, be completely
eliminated.
For design and construction of new pavements this concept means that the pavement
has to be designed and constructed in such a way that
bottom-up fatigue cracking should be prevented
rutting in the pavement layers should be avoided by using adequate asphalt
mixtures
rutting in the unbound layers and frost heave should completely eliminated.
The choice of the surface layer depends on the functional requirements. This could be
a combination of comfort, durability, stability, skid resistance and noise reduction.
There might be even additional requirements like surface water drainage or water
impermeability.
A wide range of bituminous surface layer products can be considered appropriate
depending on specific requirements. The selection of surface course is a matter of
identifying the most appropriate materials during the design life.
The bituminous binder courses should be able to withstand high shear stresses and the
bituminous base layer should be thick and stiff enough to distribute the traffic loadings
to the substrate and to withstand fatigue.
The resistance to fatigue depends on the fatigue resistance of the bituminous mixture
and the tensile strain at the bottom of the asphalt base course. The tensile strain should
be below a certain fatigue limit, under which no damage accumulates.
There are two approaches to achieve a sufficient low strain level. On approach is based
on a certain number of Equivalent Standard Axle Loads in the design and the other
approach is to limit the tensile stain at the bottom of the bituminous base layer to a
certain number:
Pavements design above a traffic level of 80 million standard axles (80 kN) are
said to be designed as long-life pavements.
Threshold values for tensile stain in the range of 50-7010
-6
m/m have been
reported as fatigue thresholds.
In practice both approaches will lead to a tensile stress level at the bottom of the
bituminous base layer that is low enough to avoid crack initiation / crack propagation.
It should be emphasised that any design parameter and criterion should not be taken
out of its context since they are closely linked to a specific design guide, test methods
used, materials used and the construction of the pavement, etc.
In the same way the maximum tensile strain at the top of the sub-grade could be
mentioned (20010
-6
m/m) to avoid rutting in the top of the subgrade.
In general the technical and functional requirements for LLP will in general be higher
compared to traditional pavements. A way to achieve this is by prescribing functional
specifications instead of technical specifications. Then it is up to the contractor to
show that a solution meets the requirements. In this way several solutions may be
considered by the contractor and the contractor will optimize the construction.
Long-Life Asphalt Pavements Technical version June 2007
18
The traditional Life Cycle Cost Analyses can be used for calculating the present worth
of costs for pavement alternatives and it is the primary tool for economic comparisons.
For Long-Life Pavement the recommended life cycle periods for short, medium and
long term analysis are in the order of 25, 50 and 100 years respectively.
6. Literature
[1.] Newcomb, D. E., Buncher, M., Huddleston, I. J. Concepts of perpetual
pavements. Transportation Research Circular, No 503, Perpetual Bituminous
Pavements, (2001).
[2.] Nunn, M. E., Brown, A., Weston, D., Nicholls, J. C. Design of long-life flexible
pavements for heavy traffic. Highways Agency, TRL report 250, (1997).
[3.] Nunn, M., Long-Life Flexible Roads, TRL, ISAP Conference 1997, Seattle
(1997)
[4.] FEHRL A guide to the use of long-life fully-flexible pavements ELLPAG
Phase I. FEHRL report 2004/01, (2004).
[5.] APA Perpetual Pavements-A Synthesis. Asphalt Pavement Alliance (APA),
published at the Asphalt Pavement Alliance homepage:
publications@asphaltalliance.com, (2002).
[6.] TRB Perpetual Bituminous Pavements. Foreword, Transportation Research
Circular, number 503, December, (2001).
[7.] Harvey, J., Long-Life AC Pavements: A Discussion of Design and construction
Criteria Based on California Experience Paper 12 Proceedings International
Symposium on Design and Construction of Long Lasting Asphalt Pavements,
Auburn USA, 7-9 June 2004.
[8.] Tseng, K. H., Lytton, R. L. Fatigue damage properties of asphaltic concrete
pavements. Transporta-tion Research Record 1286 (TRB), pp 150-163, (1990).
[9.] Sousa, J. B., Pais, J. B., Prates, M., Barros, R., Langlois, P., Leclerc, A. M.
Effect of aggregate grada-tion on fatigue life on asphalt concrete mixes.
Transportation Research Record 1630, (TRB), pp 62-68, (1997).
[10.] Tayebali, A. A., Deacon, J. A., Coplantz, J. S., Finn, F. N., Monismith, C. L.
Fatigue Response of Asphalt, Part II-Extended Test Program.SHRP Project A-
404, Asphalt Research Program, Institute of Transportation Studies, University
of California, Berkeley, (1994).
[11.] Development of New Bituminous Pavement Design Method, Final report of
COST Action 333, European Commission, Luxembourg, 1999.
[12.] Monismith, C. L., Long, F. Overlay Design for Cracked and Seated Portland
Cement Concrete (PCC) Pavement-Interstate Route 710. Technical
Long-Life Asphalt Pavements Technical version June 2007
19
Memorandum TM UCB PRC 99-3, Pavement Research Center, Institute for
Transportation Studies, University of California, Berkeley, (1999)
[13.] Timm, D.H. The Effects of Load Spectra and Variability of Perpetual Pavement
Design Paper 7 Proceedings International Symposium on Design and
Construction of Long Lasting Asphalt Pavements, Auburn USA, 7-9 June 2004.
[14.] Thompson, M., Design Principles for Long Lasting HMA Pavements Paper 14
Proceedings International Symposium on Design and Construction of Long
Lasting Asphalt Pavements, Auburn USA, 7-9 June 2004.
[15.] Peterson, R., Determination of Threshold Strain Level for Fatigue Endurance
Limit in Asphalt Mixtures Paper 15 Proceedings International Symposium on
Design and Construction of Long Lasting Asphalt Pavements, Auburn USA, 7-9
June 2004.
[16.] Lundstrom, R. Isacsson, U. An Investigation of the Applicability of Schaperys
Work Potential Model for Characterization of Asphalt Fatigue Behavior.
Published and Presented at the annual AAPT meeting, Baton Rouge, USA, mars
2004. (2004)
[17.] Robinson, R., Danielson, U., Snaith, M. Road Maintenance Management
Concepts and Systems. Macmillan Press LTD, (1998).
[18.] Lundstrom, R., Ekblad, J., Isacsson, U., Karlsson, R. Fatigue Modeling as
related to Flexible Pavement Design-State of the Art. Accepted for publication
in International Journal of Road Materials and Pavement Design, (2006)
[19.] Newcomb, D.E., A Guide to PerRoad 2.4 for PerRoad Perpetual Software
developed by Professor David H. Timm. Asphalt Pavement Alliance, August
2004. http://www.asphaltalliance.com/
[20.] Haas, R., Tighe, S. and Cowe Falls, L., Return on Investment Analysis for Long
Life Asphalt Pavements Proceedings 11
th
International Conference on asphalt
Pavements, August 12 17, 2006, Qubec City, Canada.
[21.] Harvey, J., Long, F., and Prozzi, J.A. Application of CAL/APT results to Long
Life Flexible pavement reconstruction, Accelerated Pavement Testing
Conference, Reno, NV, USA, 1999
Long-Life Asphalt Pavements Technical version June 2007
20
Appendix 1
Durability of surface layers in Europe
A.1. Introduction
Long-life Pavements or Perpetual Pavements mean building roads in such a way that
fatigue at the bottom of the asphalt pavement layer is not a critical parameter. This also
means that the total thickness of the pavement layers should be enough to avoid fatigue
starting from the bottom.
Consequently, for maintaining the road in a good condition it is sufficient to replace the
surface-layer only. In this way the durability of the surface layer is now the dominant
factor for the pavement surface life.
To get an insight into the service life of surface layers the EAPA Technical Committee
investigated the durability of the surface layers used in Europe.
This annex gives an overview of the different asphalt mix types that can be used for
surface layers and their expected durability. The data are based on a questionnaire and a
panel discussion of experts.
A.2. Asphalt mixtures
In the descriptions of the asphalt mixtures (1 to 7) the definitions are from the European
Asphalt Standards EN 13108 1 to 7 and they are quoted with inverted commas.
1. Asphaltic Concrete (AC)
Asphalt in which the aggregate particles are continuously graded or gap-graded to
form an interlocking structure. Dense asphalt concrete is often used as the basic
surface layer.
2. Asphalt Concrete for very thin layers (AC-TL)
Asphalt for surface courses with a thickness of 20 mm to 30 mm, in which the
aggregate particles are generally gap-graded to form a stone to stone contact and to
provide an open surface texture. This mixture is often used in France and is called
BBTM (Bton Bitumineuse Trs Mince).
3. Soft Asphalt (SA)
Mixture of aggregate and soft bitumen grades. This flexible mixture is used in the
Nordic countries for secondary roads.
4. Hot Rolled Asphalt (HRA)
Dense, gap graded bituminous mixture in which the mortar of fine aggregate, filler
and high viscosity binder are major contributors to the performance of the laid
material. Coated chippings (nominally single size aggregate particles with a high
resistance to polishing, which are lightly coated with high viscosity binder) are always
rolled into and form part of a Hot Rolled Asphalt surface course. This durable surface
layer was often used as a surface layer in the UK.
Long-Life Asphalt Pavements Technical version June 2007
21
5. Stone Mastic Asphalt (SMA)
Gap-graded asphalt mixture with bitumen as a binder, composed of a coarse crushed
aggregate skeleton bound with a mastic mortar. This mixture is of often used as a
surface layer in case high stability is needed. The surface structure also has good noise
reducing properties.
6 Mastic Asphalt (MA)
Voidless asphalt mixtures with bitumen as a binder in which the volume of filler and
binder exceeds the volume of the remaining voids in the mixed. This mixture is very
durable and was often used as surface layer in certain countries.
7. Porous Asphalt (PA)
Bituminous material with bitumen as a binder prepared so as to have a very high
content of interconnected voids which allow passage of water and air in order to
provide the compacted mixture with drain and noise reducing characteristics.
8. Double layered Porous Asphalt (2L-PA)
The top layer with a grain size 4/8 mm is about 25 mm thick and the second/bottom
layer is porous asphalt with a course aggregate (11/16 mm). The total thickness is about
70 mm. Because of the finer texture at the top (that gives less tyre vibrations), it gives a
better noise reduction than a single layer porous asphalt.
9. Asphalt Concrete for ultra thin layers (UTLAC)
Asphalt for surface courses with a thickness of 10 mm to 20 mm, in which the
aggregate particles are generally gap-graded to form a stone to stone contact and to
provide an open surface texture. Several varieties of this layer are often used to provide
a good, new noise reducing surface layer.
The difference between the mixtures with regard to structure and skeleton are also
illustrated in figures 5, 6 and 7.
Figure 5: Difference in structure between AC, SMA, BBTM and PA.
Long-Life Asphalt Pavements Technical version June 2007
22
Figure 6: Difference between sand skeleton and stone skeleton mixtures
Figure 7: Structure of double- layered Porous Asphalt
A.3. Basic assumptions for determining the durability of the surface layers
The expected durability is based on the best practice. This means that surface layers are
expected to be laid on a properly designed road where the durability of the surface layer is
not determined by bottom-up fatigue cracking.
Also, it is assumed that the mix is properly designed and well compacted. As an example,
a SMA surface layer that shows rutting in the SMA is an improperly designed mixture.
The data shown are not valid in the case of using studded tyres.
The durability of surface layers also depends on the local conditions, the local climate, the
mix formula, the types of bitumen and aggregate used, the maximum allowable axle loads
and the actual axle loads used (because excessively high axle loads have a strong negative
influence on the service life of the pavement surface layers). In some cases or countries
the skid resistance of the surface layer is the dominant factor for determining the service
life, so the durability depends on the required friction level and the PSV-value of
aggregate that has been used.
A distinction has been made between major roads (motorways and heavily traffic roads)
and secondary roads.
Long-Life Asphalt Pavements Technical version June 2007
23
A.4. Results
Table 1 and Figure 8 show the Durability of Surface Layers is expressed in years of
service life for major roads / motorways / heavily trafficked roads.
Table 2 and Figure 9 show the Durability of Surface Layers is expressed in years of
service life for secondary roads.
Major roads / motorways / heavily trafficked
Type 15% Lowel level European average 85% Higher level
AC 8 14 18
AC-TL 30-40
mm 8 12 18
AC-VTL 25-30
mm 8 10 12
UTLAC 8 10 12
PA 8 10 14
2L-PA
1
) 9 11 12
SMA 14 20 25
HRA 17 21 25
Mastic-A 18 21 24
Soft-A is not used here
1
) Only based on Dutch results
Table 1: Durability of surface layers on major roads
Major roads / Motorways / Heavily trafficked roads
0
5
10
15
20
25
30
AC AC-TL AC-VTL UTLAC PA 2L-PA SMA HRA Mastic-A
Surface layer type
Y
e
a
r
s
15% Lowel level
85% Higher level
European average
Figure 8: Durability of surface layers on major roads
Long-Life Asphalt Pavements Technical version June 2007
24
Secondary roads
Type 15% Lowel level European average 85% Higher level
AC 10 15 20
AC-TL 10 15 20
AC-VTL 10 12 14
2L-PA
1
) 10 11 12
SMA 16 20 25
HRA 20 25 30
Mastic-A 18 24 30
Soft-A 8 12 25
PA and UTLAC are not used here
1
) Only based on Dutch results
Table 2: Durability of surface layers on secondary roads
Secondary roads
0
5
10
15
20
25
30
35
AC AC-TL AC-VTL 2L-PA SMA HRA Mastic-A Soft-A
Surface layer type
Y
e
a
r
s
15% Lowel level
85% Higher level
European average
Figure 9: Durability of surface layers on secondary roads