Fomapan 200
Fomapan 200
Fomapan 200
DEVELOPING INSTRUCTIONS
Foma B&W film is compatible with all major processing systems. Recommended developing times are
for normal contrast negatives (based on intermittent agitation.) All developing times are standardized
for 68F / 20C. Your developing time may vary based on environment and equipment used.
DEVELOPER DILUTION TIME @ 68F / 20C
Arista
76 Powder Stock 5 - 6
Arista
76 Powder 1:1 8 - 9
Arista
Wavelength [nm]
Characteristic curves
Exposure: Daylight (5500 K), 1/20 s
Developer: Microphen at 20
o
C
3
2
1
-3
0
1
2
3
-2 -1 0
14 min
2 6 min
3 8 min
O
p
t
i
c
a
l
d
e
n
s
i
t
y
Log rel. exposure
Modulation transfer function
Resolving power
110 lines per mm
Granularity
RMS = 14,0 (Microphen at 20
o
C, developed to G = 0,6.
Measured at D = 1,0.
Base
The following bases are used for manufacturing the particular sorts of the film:
- 120 rollfilm - a bluish polyester base 0,1 mm thick, furnished with a matted colour
backing which will decolourize during processing. The backing has anti-halation and
anti-curling properties and prevents the incidence of Newton rings during enlarging.
- 35 mm film - a gray or gray-blue cellulose triacetate base 0,135 mm thick,
- sheet film - a clear polyester base 0,175 mm thick furnished with a matted colour
backing which will decolourize during processing. The backing has anti -halation and
anti-curling properties and prevents the incidence of Newton rings during enlarging.
FOMAPAN 200 Creative
BLACK-AND-WHITE NEGATIVE FILM
The product has been produced and marketed in conformity
with a quality system according to the international standard
ISO 9001.
Spatial frequency [lines per mm]
FOMA 7/02
FOMA 501 04 Hradec Krlov Tel.: +420 495 733 258 export@foma.cz
Bohemia Ltd. Czech Republic Fax: +420 495 733 376 www.foma.cz
DEVELOPMENT CURVES FOR FOMAPAN 200 Creative
0,10
0,20
0,30
20
o
C
0,4
0,6
0,8
1,0
1,2
0,4
0,6
0,8
1,0
1,2
0,4
0,5
0,6
0,7
0,8
0,4
0,6
0,8
1,0
1,2
D
min
S
( )
o
ISO ( )
o
ISO
( )
o
ISO ( )
o
ISO
200
160
125
100
80
200
160
125
100
80
200
160
125
100
80
200
160
125
100
80
200
160
125
100
80
200
160
125
100
80
160
125
100
80
200
160
125
100
80
S
S
S
S
S
S
S
D
min
D
min
D
min
S
6 8 4 10
t (min)
6 8 4 10
t (min)
5 7 3 9
t (min)
6 8 4 10
t (min)
0,00
0,10
0,20
20
o
C
S
0,10
0,20
0,30
20
o
C
S
30
o
C
0,10
0,20
0,30
1 2 4 3 5 t (min)
1 2 4 3 5 t (min)
1 2 4 3 5 t (min)
1 2 4 3 5 t (min)
S
0,4
0,6
0,8
1,0
1,2
G
G
G
G
G
G
G
G
G
G
G
G
G
G
G
G
0,4
0,6
0,8
1,0
1,2
0,4
0,6
0,8
1,0
1,2
0,4
0,6
0,8
1,0
1,2
D
min
D
min
D
min
D
min
30
o
C
0,00
0,10
0,20
S
30
o
C
0,10
0,20
0,30
S
30
o
C
0,10
0,20
0,30
S
0,10
0,20
0,30
20
o
C
S
( )
o
ISO ( )
o
ISO
( )
o
ISO ( )
o
ISO
Ilford ID 11stock
Kodak D 76 developer
Fomadon Excel
Kodak Xtol developer
Fomadon LQN developer (1+10)
Ilford Microphen developer
D /S/G development time curves at 20
and 30 C
- daylight Tc = 5500 K
- spiral developing tank - agitation or
turning over continuously during the first
30 seconds, then during the first 10
seconds in every minute.
min
o
D /S/G development time curves at 20
and 30 C
- daylight Tc = 5500 K
- spiral developing tank - agitation or
turning over continuously during the first
30 seconds, then during the first 10
seconds in every minute.
min
o
D /S/G development time curves at 20
and 30 C
- daylight Tc = 5500 K
- spiral developing tank - agitation or
turning over continuously during the first
30 seconds, then during the first 10
seconds in every minute.
min
o
D /S/G development time curves at 20
and 30 C
- daylight Tc = 5500 K
- spiral developing tank - agitation or
turning over continuously during the first
30 seconds, then during the first 10
seconds in every minute.
min
o