1. Scope
1.1 This test method provides a procedure for the determination of the water absorption by a core of concrete taken from
a surface treated with a water repellent.
1.2 The intended use of the water repellent coating is to
reduce the amount of water that absorbs into the substrate.
1.3 The values stated in SI units are to be regarded as the
standard. The values given in parentheses are for information
only.
1.4 This standard does not purport to address all of the
safety concerns, if any, associated with its use. It is the
responsibility of the user of this standard to establish appropriate safety and health practices and determine the applicability of regulatory limitations prior to use.
2. Referenced Documents
2.1 ASTM Standards:
C 42 Test Method for Obtaining and Testing Drilled Cores
and Sawed Beams of Concrete2
D 1193 Specification for Reagent Water3
D 1763 Specification for Epoxy Resins4
D 3924 Specification for Standard Environment for Conditioning and Testing Paint, Varnish, Lacquer, and Related
Materials5
E 145 Specification for Gravity Convection and Force Ventilation Ovens6
E 898 Test Method of Testing Top Loading, Direct Reading
Laboratory Scales and Balances6
1
This test method is under the jurisdiction of ASTM Committee D01 on Paint
and Related Coatings, Materials, and Applications and is the direct responsibility of
Subcommittee D01.47 on Masonry Treatments.
Current edition approved Dec. 10, 1999. Published February 2000.
2
Annual Book of ASTM Standards, Vol 04.02.
3
Annual Book of ASTM Standards, Vol 11.01.
4
Annual Book of ASTM Standards, Vol 08.01.
5
Annual Book of ASTM Standards, Vol 06.01.
6
Annual Book of ASTM Standards, Vol 14.04.
6. Sealing Material
6.1 Use hardened concrete specimens as described in 7.1.
Copyright ASTM International, 100 Barr Harbor Drive, PO Box C700, West Conshohocken, PA 19428-2959, United States.
D 6489 99
6.2 Follow the procedures of Section 8, except for 8.4 and
8.5. Instead use the sealing material to completely seal the
specimen, top, bottom and sides.
6.3 Follow the procedures of Section 9, except completely
submerged the specimens so that the water level is 25.4 mm
(1.0 in.) over the top of the specimen.
6.4 After the specimens have been submerged in water for
48 h, acceptable sealing materials shall have a percent absorption of less then 0.1 %.
7. Test Specimen
7.1 Typical test specimens are hardened concrete cores,
approximately 7.0 cm (2.75 in.) in diameter and 7.5 cm (2 to 3
in.) in length. A minimum of three cores for each test shall be
used. Cores should be pulled in such a manner as not to
damage the integrity of the surface. See Test Method C 42 for
guidance.
9. Procedure
9.1 Weight each specimen to the nearest 0.1 g and record
weight as W1.
9.2 Place specimens treated or exposed side of specimens
face down in container. Specimens should be placed on glass
rods that are in the bottom of container so water is free to
circulate under the specimens.
9.3 Fill container with reagent grade water until level is 6.4
cm (2.5 in.) from the top of the glass rods. Water shall not come
in contact with opposite face of the core.
9.4 Soak the cores for 48 h. At the 24 and 48-h immersion
period, remove the specimens from the water and wipe with a
damp cloth and weight to the nearest 0.1 g and record as W2.
9.5 Determine the percent of water absorbed by each
specimen as follows:
8. Preparation of Specimens
8.1 Clean the sides and both faces of the specimens of all
loose dust or cement paste from the core drilling process. Use
compressed air or water and a soft brush only, more vigorous
cleaning methods may damage some water repellent coatings.
8.2 Dry the specimens in a forced draft oven for 24 h at
75C 6 5C (167 F 6 9F) until two successive weighings at
intervals of 2 h show an increment of loss not greater than
0.2 % of the last previously determined weight.
8.3 After drying, remove the specimens from the oven and
allow them to cool to room temperature under ambient
conditions (see Specification D 3924). Weigh each specimen to
the nearest 0.1 g and record weight as WA.
8.4 Prepare sufficient wax or epoxy material to adequately
coat all the specimens. If using wax, melt enough in a suitable
container or if using a two-component coating, mix quantities
that can be applied during the pot-life of the coating.
8.5 To keep the sealing material from contaminating the
treated top surface and the bottom untreated surface of the
specimen, place duct tape over these areas and cut the tape
around the circumference so that there is no overlap on the
longitudinal sides of the core.
8.6 Apply the sealing material to the specimens by either
placing the longitudinal side of the specimen in the sealing
material (place enough sealing material in the container so it is
at least to a depth of 6.4 mm (0.25 in.)) and roll the specimen
two to three revolutions, or brush on the sealing material. Be
careful not to get any of the sealing material on the treated face.
8.7 Remove the specimen from the sealing material and
place treated specimen face up on a firm surface.
Percent Absorption 5
(1)
10. Report
10.1 Report the following information:
10.1.1 Type and size of concrete specimens.
10.1.2 Water repellent treatment used, application rate and
method of application.
10.1.3 Percent water absorption of each specimen, and
10.1.4 Any deviation from this procedure.
11. Precision and Bias
11.1 PrecisionPrecision for this test method has not been
determined at this time.
11.2 BiasBias for this test method cannot be determined
since there is no reference standard available for comparison.
12. Keywords
12.1 field treatment evaluation; water absorption; water
repellent
D 6489 99
ASTM International takes no position respecting the validity of any patent rights asserted in connection with any item mentioned
in this standard. Users of this standard are expressly advised that determination of the validity of any such patent rights, and the risk
of infringement of such rights, are entirely their own responsibility.
This standard is subject to revision at any time by the responsible technical committee and must be reviewed every five years and
if not revised, either reapproved or withdrawn. Your comments are invited either for revision of this standard or for additional standards
and should be addressed to ASTM International Headquarters. Your comments will receive careful consideration at a meeting of the
responsible technical committee, which you may attend. If you feel that your comments have not received a fair hearing you should
make your views known to the ASTM Committee on Standards, at the address shown below.
This standard is copyrighted by ASTM International, 100 Barr Harbor Drive, PO Box C700, West Conshohocken, PA 19428-2959,
United States. Individual reprints (single or multiple copies) of this standard may be obtained by contacting ASTM at the above
address or at 610-832-9585 (phone), 610-832-9555 (fax), or service@astm.org (e-mail); or through the ASTM website
(www.astm.org).