Location via proxy:   [ UP ]  
[Report a bug]   [Manage cookies]                

Mix Design Report - Malkangiri-311

Download as pdf or txt
Download as pdf or txt
You are on page 1of 1

Indian Institute of Technology Bhubaneswar

Aragul, Jatni, Odisha-752050

SCHOOL OF INFRASTRUCTURE
No. IITBBS/SIF/CP104/Malkangiri/21             Date:  18.05.2018 
 
Client: Rural Works Sub‐Division, Malkangiri, Odisha 
Reference: Your Letter No. 534 dated 15.02.2018 
Description: Mix design for cement treated Sub‐base and Base for Roads (Road:MV‐53 to Semiliguda 
in Package No. OR 20‐311) under PMGSY  
TEST RESULTS 
The following are the results obtained from various Tests conducted on the samples supplied by the 
client for Cement Treated Subbase and Base Construction. 
 
Sample: Moorum (Lateritic Soil/Gravel) and Cement (ACC PSC)     
A. Soil Characterization: 
Sl. No.  Property  Value 
1  Grain Size Distribution (wet sieve analysis)   
  Gravel Size (%)  37 
  Sand Size (%)  44 
  Fines (%)  19 
2  Index Properties   
  Liquid Limit  37 
  Plastic Limit  25 
  Plasticity Index  12 
3  Soil Classification (as per IS)  SC 
B. Compaction Characteristics of the Cement Stabilized Mix: 
Sl No.  Property  Cement Content (% by weight) 
4%  8% 
1  OMC (%)  8.6  8.9 
3
2  MDD (kN/m )  22.8  22.8 
C. Strength Characteristics of the Cement Stabilized Mix: 
Sl No.  Property  Cement Content (% by weight) 
4%  8% 
1  Unconfined Compressive Strength  2.23  4.25 
after 7‐days of Curing (MPa) 
Recommendations: Based on the above results, it is recommended to add 4% cement by weight of 
mix for construction of cement treated subbase and 8% by weight for cement treated base layer to 
achieve the desired strength. About 20% stone aggregates in base layer may be added for better 
performance. Quality of cement and date of packing should be thoroughly checked before use for 
stabilization. Use vibratory roller for better output. 

 
(Dr. U. C. Sahoo) 

 
 