Unit 1 - Basic Civil Engineering & Engineering Mechanics - WWW - Rgpvnotes.in

Download as pdf or txt
Download as pdf or txt
You are on page 1of 18

Program : B.

Tech
Subject Name: Basic Civil Engineering & Mechanics
Subject Code: BT-204
Semester: 2nd
Downloaded from be.rgpvnotes.in

Subject Name: Basic Civil Engineering & Engineering Mechanics Subject Code: BT-2004

Unit: 01
BUILDING MATERIALS:
1. Bricks: Manufacturing, field and laboratory test, Engineering properties.
2. Cement: Types, physical properties, laboratory tests
3. Concrete and Mortar Materials: Workability, Strength Properties of Concrete, Nominal
proportion of Concrete, Preparation of Concrete, Compaction Curving.
Mortar: Properties and Uses.

Bricks:
Properties:
All properties of brick are affected by raw material composition and the manufacturing
process. Most manufacturers blend different clays to achieve the desired properties of the
raw materials and of the fired brick. This improves the overall quality of the finished product.
The quality control during the manufacturing process permits the manufacturer to limit
variations due to processing and to produce a more uniform product. The most important
properties of brick are 1) durability, 2) color, 3) texture, 4) size variation, 5) compressive
strength and 6) absorption.
Durability
The durability of brick depends upon achieving incipient fusion and partial vitrification during
firing. Because compressive strength and absorption values are also related to the firing
temperatures, these properties, together with saturation coefficient, are currently taken as
predictors of durability in brick specifications. However, because of differences in raw
materials and manufacturing methods, a single set of values of compressive strength and
absorption will not reliably indicate the degree of firing.
Color
The color of fired clay depends upon its chemical composition, the firing temperatures and
the method of firing control. Of all the oxides commonly found in clays, iron probably has the
greatest effect on color. Regardless of its natural color, clay containing iron in practically any
form will exhibit a shade of red when exposed to an oxidizing fire because of the formation of
ferrous oxide. When fired in a reducing atmosphere, the same clay will assume a dark (or
black) hue. Creating a reducing atmosphere in the kiln is known as flashing or reduction firing.
Given the same raw material and manufacturing method, darker colors are associated with
higher firing temperatures, lower absorption values and higher compressive strength values.
However, for products made from different raw materials, there is no direct relationship
between strength and color or absorption and color.
Texture, Coatings and Glazes
Many brick have smooth or sand-finished textures produced by the dies or molds used in
forming. Smooth textures, commonly referred to as a die skin, results from pressure exerted
by the steel die as the clay passes through it in the extrusion process. Most extruded brick
have the die skin removed and the surface further treated to produce other textures using
devices that cut, scratch, roll, brush or otherwise roughen the surface as the clay column
leaves the die (see Photo 6).

Page no: 1 Follow us on facebook to get real-time updates from RGPV


Downloaded from be.rgpvnotes.in

Subject Name: Basic Civil Engineering & Engineering Mechanics Subject Code: BT-2004

Figure: Some Brick Textures are applied by Passing under a Roller after Extrusion
Size Variation
Because clays shrink during both drying and firing, allowances are made in the forming
process to achieve the desired size of the finished brick. Both drying shrinkage and firing
shrinkage vary for different clays, usually falling within the following ranges:
• Dr i g shri kage: to per e t
• Firi g shri kage: . to per e t
Firing shrinkage increases with higher temperatures, which produce darker shades. When a
wide range of colors is desired, some variation between the sizes of the dark and light units is
inevitable. To obtain products of uniform size, manufacturers control factors contributing to
shrinkage. Because of normal variations in raw materials and temperature variations within
kilns, absolute uniformity is impossible. Consequently, specifications for brick allow size
variations.

Compressive Strength and Absorption


Both compressive strength and absorption are affected by properties of the clay, method of
manufacture and degree of firing. For a given clay and method of manufacture, higher
compressive strength values and lower absorption values are associated with higher firing
temperatures. Although absorption and compressive strength can be controlled by
manufacturing and firing methods, these properties depend largely upon the properties of
the raw materials.

Rail kilns

In modern brickworks, this is usually done in a continuously fired tunnel kiln, in which the
bricks are fired as they move slowly through the kiln on conveyors, rails, or kiln cars, which
achieves a more consistent brick product. The bricks often have lime, ash, and organic matter
added, which accelerates the burning process.

Page no: 2 Follow us on facebook to get real-time updates from RGPV


Downloaded from be.rgpvnotes.in

Subject Name: Basic Civil Engineering & Engineering Mechanics Subject Code: BT-2004

Bull's Trench Kilns

In India, brick making is typically a manual process. The most common type of brick kiln in use
there is the Bull's Trench Kiln (BTK), based on a design developed by British engineer W. Bull
in the late 19th century.

Figure 2: Bull's Trench Kiln

An oval or circular trench is dug, 6–9 meters wide, 2-2.5 meters deep, and 100–150 meters in
circumference. A tall exhaust chimney is constructed in the centre. Half or more of the trench
is filled with "green" (unfired) bricks which are stacked in an open lattice pattern to allow
airflow. The lattice is capped with a roofing layer of finished brick. In operation, new green
bricks, along with roofing bricks, are stacked at one end of the brick pile; cooled finished
bricks are removed from the other end for transport to their destinations. In the middle, the
brick workers create a firing zone by dropping fuel (coal, wood, oil, debris, and so on) through
access holes in the roof above the trench. The advantage of the BTK design is a much greater
energy efficiency compared with clamp or scove kilns. Sheet metal or boards are used to
route the airflow through the brick lattice so that fresh air flows first through the recently
burned bricks, heating the air, then through the active burning zone. The air continues
through the green brick zone (pre-heating and drying the bricks), and finally out the chimney,
where the rising gases create suction which pulls air through the system. The reuse of heated
air yields savings in fuel cost.

Page no: 3 Follow us on facebook to get real-time updates from RGPV


Downloaded from be.rgpvnotes.in

Subject Name: Basic Civil Engineering & Engineering Mechanics Subject Code: BT-2004

As with the rail process above, the BTK process is continuous. A half dozen laborers working
around the clock can fire approximately 15,000–25,000 bricks a day. Unlike the rail process, in
the BTK process the bricks do not move. Instead, the locations at which the bricks are loaded,
fired, and unloaded gradually rotate through the trench.

Use

Bricks are used for building, block paving and pavement. Bricks in the metallurgy and glass
industries are often used for lining furnaces, in particular refractory bricks such as silica,
magnesia, chamotte and neutral (chromo magnesite) refractory bricks. This type of brick
must have good thermal shock resistance, refractoriness under load, high melting point, and
satisfactory porosity. Engineering bricks are used where strength, low water porosity or acid
(flue gas) resistance are needed.

Cement

Cement is the product obtained by burning a well-proportioned mixture of silicious,


argillaceous and calcareous materials and crushing the same into a fine powder. In the most
general sense of the word, cement is a binder, a substance that sets and hardens

Page no: 4 Follow us on facebook to get real-time updates from RGPV


Downloaded from be.rgpvnotes.in

Subject Name: Basic Civil Engineering & Engineering Mechanics Subject Code: BT-2004

independently, and can bind other materials together. The word "cement" traces to the
Romans, who used the term opus caementicium to describe masonry resembling modern
concrete that was made from crushed rock with burnt lime as binder. The volcanic ash and
pulverized brick additives that were added to the burnt lime to obtain a hydraulic binder
were later referred to as cementum, cimentum, cäment, and cement.

Cements used in construction can be characterized as being either hydraulic or non-hydraulic.


Hydraulic cements (e.g., Portland cement) harden because of hydration, a chemical reaction
between the anhydrous cement powder and water. Thus, they can harden underwater or
when constantly exposed to wet weather. The chemical reaction results in hydrates that are
not very water-soluble and so are quite durable in water. Non-hydraulic cements do not
harden underwater; for example, slaked limes harden by reaction with atmospheric carbon
dioxide.

The most important uses of cement are as an ingredient in the production of mortar in
masonry, and of concrete, a combination of cement and an aggregate to form a strong
building material. In 1824, Joseph Aspdin patented a material, which he called Portland
cement, because the render made from it was in color similar to the prestigious Portland
stone.

Types of cement

1. Ordinary Portland cement (OPC – IS 269): Cement is made by heating limestone


(calcium carbonate) with small quantities of other materials (such as clay) to 1450 °C
in a kiln, in a process known as calcination, whereby a molecule of carbon dioxide is
liberated from the calcium carbonate to form calcium oxide, or quicklime, which is
then blended with the other materials that have been included in the mix. The
resulting hard substance, called 'clinker', is then ground with a small amount of
gypsum into a powder to make 'Ordinary Portland Cement', the most commonly used
type of cement (often referred to as OPC). Portland cement is a basic ingredient of
concrete, mortar and most non-specialty grout. The most common use for Portland
cement is in the production of concrete. Concrete is a composite material consisting of
aggregate (gravel and sand), cement, and water. As a construction material, concrete
can be cast in almost any shape desired, and once hardened, can become a structural
(load bearing) element. Portland cement may be grey or white.

The Portland cement consists of the following components:

1) Lime 60% to 67%.


2) Silica 17% to 25%.
3) Alumina 03% to 08%.
4) Iron oxide 0.50% to 06%.
5) Magnesia 0.10% to 04%.
6) Soda and Potash 0.20% to 01%.

Page no: 5 Follow us on facebook to get real-time updates from RGPV


Downloaded from be.rgpvnotes.in

Subject Name: Basic Civil Engineering & Engineering Mechanics Subject Code: BT-2004

7) Sulphur Trioxide 01% to 2.75%.


8) Free Lime 0% to 1%.

Cement is a complicated mixture of chemical compounds. Ordinary Portland cement contains


the following compounds:

1) Tri calcium silicate (Ca O) 3 SiO2 denoted by C3S.


2) Di calcium silicate (Ca O) 2 SiO2 denoted by C2S.
3) Tri calcium Aluminate (Ca O) 3 Al2O3 denoted by C3A.
4) Tetra calcium Alumino ferrite (Ca O) 4 Al2O3 Fe2O3 denoted by C4AF.

About 70% to 80% of cement is contributed by C3S and C2S which are responsible for the
strength of cement. These compounds provide to cement the property to resist the attacks of
acids and alkalis and make the cement durable. Tri calcium silicate has the property of
hydrating rapidly and is responsible to provide not only early strength but also ultimate
strength. Di calcium silicate has the property of hydrating less rapidly and provides the
strength after duration of 7 days. Tri calcium Aluminate gets hydrated rapidly and is also
responsible to provide early strength but is found to slightly retard the ultimate strength. The
compound is susceptible to be attacked by alkalis and salts. Tetra calcium Alumino ferrite
appears to be redundant not known to provide any strength and is at times considered as an
undesirable compound which gets into cement.

2. Rapid hardening Portland cement

This type of cement is manufactured in a manner similar to that of ordinary Portland cement,
but it differs in respect of chemical composition, degree of burning and grinding. This
contains greater lime content than ordinary Portland cement. This requires a better control of
burning the ingredients over a longer period of time. The clinker is ground to a much finer
extent than the ordinary Portland cement. The quick rate of gain of strength is due to a
higher content of Tri calcium silicate and finer grinding of clinker. For the same water cement
ratio, it gains strength in 3 days what the ordinary Portland cement gains in 7 days; and it
gains a strength in 7 days what the ordinary cement gains in 28 days. The main advantage in
using rapid hardening Portland cement is that the shuttering may be struck considerably
earlier, thus saving considerable time and expenses. This cement is particularly satisfactory
under conditions of frost. This cement can also be used for road work, so that the road can be
open to traffic with least delay.

3. Low Heat Portland cement

During the process of setting and hardening of cement, an appreciable rise of temperature
occurs. The heat generated in ordinary cement at the end of 3 days may be at the order of 80
calories per gram of cement. In massive constructions like abutments, retaining walls, dams
etc. the rate at which the heat can be lost at the surface is lower than at which the heat is
initially generated. The temperature rise is an important factor, because the shrinking which

Page no: 6 Follow us on facebook to get real-time updates from RGPV


Downloaded from be.rgpvnotes.in

Subject Name: Basic Civil Engineering & Engineering Mechanics Subject Code: BT-2004

may take place during the cooling processes introduces tensile stresses in concrete. This will
therefore affect the water tightness of the structure and may lead to deterioration. In low
heat cement the heat involved is less. As per the code the heat of hydration for low heat
cement shall not exceed 65 calories per gram of cement at 7 days, 75 calories per gram of
cement at 28 days. The strength of this cement is a little lower than that of ordinary cement
during the first two or three months, but its strength after this period is practically the same
as that of ordinary cement. This cement offers better resistance to chemical deterioration
than ordinary Portland cement.

Low heat cement is obtained by increasing Di calcium silicate content, decreasing Tri calcium
silicate content and considerably bringing down Tri calcium Aluminate. The lesser rate of gain
of strength in the initial period is due to the reduction of Tri calcium silicate and Tri calcium
Aluminate. However, in order the rate of gain of strength may be ensured sufficiently, the IS
code recommends a specific surface requirement of 3200 cm 2/gm.

4. Portland Blast Furnace cement (IS 455)

This is the cement obtained by inter grinding Portland cement clinker with blast furnace slag.
The blast furnace slag content shall not exceed 65%. The property of cement is not detracted
by the above blending. On the contrary, the blending provides some advantages. The
granulated slags possess latent hydraulic properties which are activated to a great extent
when the slag is catalyzed and inter ground with Portland cement clinker. This cement can be
used at all places where OPC is used. In addition due to low heat evolution it can be used in
huge mass concrete structures like dams, retaining walls, foundations and abutment of
bridges. This cement has a good Sulphate resistance and is very suitable for use in
construction in sea water.

5. Portland Pozzolana cement (IS 1489)

This cement is made either by inter grinding Portland clinker and pozzolana or uniform
blending Portland cement and fine pozzolana. Inter grinding does not present any difficulty
whereas, blending tends to produce a non-uniform product. The IS code has suggested that
the latter method may be confined to factories where intimate blending can be guaranteed
through mechanical means.

The pozzolana content varies from 10% to 25% by weight of cement. Pozzolanas do not
possess cementing value themselves but have the property of combining with lime to
produce a stable lime Pozzolana compound which possesses cementing property. Since the
free lime which is readily attacked chemically is removed, the pozzolana concretes have a
greater resistance to chemical agencies. They can also resist attack by sea water better than
OPC since pozzolana cement has a lower heat evolution and is properly used in the
construction dams. The pozzolana used in the manufacture of cement in India consists of
burnt clay of shale or flyash. The pozzolana must satisfy very strictly certain requirements in

Page no: 7 Follow us on facebook to get real-time updates from RGPV


Downloaded from be.rgpvnotes.in

Subject Name: Basic Civil Engineering & Engineering Mechanics Subject Code: BT-2004

order to use it successfully. The following table shows the compressive strengths reached by
ordinary Portland cement and Portland pozzolana cement.

Age in days Compressive strength in N/mm2.


Ordinary Portland
Portland cement Pozzolana
cement
1 8 8
3 19 16
7 26 25
14 31 30
15 38 38

6. White cement:

White cement has practically the same composition and has the same strength as OPC. To
obtain the white color the iron oxide content is reduced considerably (about 1%). The raw
materials for this cement are lime stone, and china clay with low iron content. Sometimes
cryolite (Sodium alumino fluoride) is added as a flux to aid in burning. The cement is burnt in
rotary kiln with coal as fuel. This cement is used as a base for colored cement. It is used for
interior and exterior decorative works, facing works, flooring works, ornamental concrete
products, paths of garden, swimming pools etc.

7. Colored cement:

Colored cement is obtained by adding 5% to 10% of ground pigments to OPC. The following
table gives the pigments generally used to get different colors.

Desired color Pigment used


Green Chromium oxide or greenish blue ultra-marine
Blue Ultra marine
Blue black Carbon black
Black Black oxide of Manganese
Red Red oxide of iron.

8. Sulphate resisting cement:

This cement is similar to OPC, but in this case it contains greater proportion of Tri calcium
silicate and Di calcium silicate and a low content of Tri calcium Aluminate and tetra calcium
Alumino ferrite. The chemical combination of Tri calcium Aluminate and tetra calcium
Alumino ferrite renders the cement resistant to Sulphate. This type of cement is particularly
useful in the airid western regions of India where the water deposits a large amount of
sulphates in the soil.

Page no: 8 Follow us on facebook to get real-time updates from RGPV


Downloaded from be.rgpvnotes.in

Subject Name: Basic Civil Engineering & Engineering Mechanics Subject Code: BT-2004

9. Hydrophobic cement:

This is special type cement manufactured by the Associated Cement Company (ACC) which is
claimed to have the property of repelling water. Hence the cement stored or transported
does not spoiled even during the monsoons. This cement is made by adding water repellant
chemicals to ordinary Portland clinkers in the process of grinding. The chemicals added form
a molecular coating over every grain of cement and thus prevent any absorption of moisture
from air by the cement. In concreting process, in the mixer, the coating gets removed by
abrasion.

10. Oil well cement:

After the oil well is dug, it is necessary to fill the clearance between the steel lining and the
wall of the well. It is necessary to grout the porous strata so that the wall of the well is
prevented from collapse. It is also necessary to keep the ground waters out of the shaft of the
well. Oil wells are dug to great depths (1000 m to 5000 m) and at high temperatures. Thus in
such conditions the cement used for sealing the oil wells be in such a state, the slurry if
pumped into the well casing will remain in the fluid state for a few hours before it can
harden. For such a condition ACC have manufactured the oil well cement which is designed to
be best suited for sealing the deep oil wells at temperature not exceeding 100 °C.

11. Air entrant cement:

In this case indigenously air entraining agents like glues, resins, sodium salts etc. are added
while grinding the clinker. This cement provides greater workability of concrete at lesser
water cement ratio. This cement increases the frost resisting capacity of concrete.

Physical requirements for cement (IS 269, 455, 1489)

The following table gives the physical requirements for cement.

Type of cement Ordinary Rapid Low heat Blast Portland


Portland hardening PC furnace slag pozzolana
cement PC cement cement
Fineness-Residue by ≤ % ≤ % --- ≤ % ≤ %
weight on 90µ IS sieve
minimum specific 2250 3250 3200 2250 3000
2
surface cm /gm
Soundness expansion ≤ ≤ ≤ ≤ ≤
(Le Chatelier)
Setting time Initial ≤
Final i ≤ ≤ i ≤ i ≤ i ≤ i
600 min ≤ i ≤ i ≤ i ≤ i

Page no: 9 Follow us on facebook to get real-time updates from RGPV


Downloaded from be.rgpvnotes.in

Subject Name: Basic Civil Engineering & Engineering Mechanics Subject Code: BT-2004

Minimum compressive
strength (N/mm2)
1 day 3 --- 16 --- --- ---
days 7 16 28 10 16 ---
days 14 22 --- 16 22 18
days 28 --- --- --- --- 25
days --- --- 35 --- ---
Heat of Average
hydration drying
not to shrinkage
exceed of mortar
65cal/gm is not to
at 7 days exceed
and 0.15%.
75cal/gm
at 28 days

Chemical requirements for cement (IS 269, 455, 1489)

The following table gives the physical requirements for cement.

Type of cement Ordinary and Low heat Blast Portland


rapid PC furnace pozzolana
hardening slag cement
Portland cement
cement
Maximum Permissible value
Insoluble residue 15% 15% 1.5% x+{1.5(100-
x)/100}
x=declared
percentage of
pozzolana in the
cement.
Magnesia (MgO) 6% 6% 8% 5%
Sulphor as SO3 2.75% 2.75% 3% 2.75%
Sulphor as sulphide -- -- 1.5% --
Oxide of Manganese
(Mn2O3) -- -- 2% --
Ignition loss 4% 4% 4% 5%

Role of various ingredients of cement


The various ingredients in cement have their characteristic functions.

Page no: 10 Follow us on facebook to get real-time updates from RGPV


Downloaded from be.rgpvnotes.in

Subject Name: Basic Civil Engineering & Engineering Mechanics Subject Code: BT-2004

Silica provides strength to cement. Excess silica may enhance the strength but increases the
setting time.
Lime also provides strength to cement. Excess of lime is resulting in objectionable expansion.
Insufficient lime reduces the strength and decreases the setting time.
Alumina makes the cement quick setting. It brings down the clinking temperature acting as a
flux. Excess of this ingredient lowers the strength.
Iron oxide provides colour to the cement. This also imparts strength and hardness to the
cement.
Magnesia when present in small extent provides hardness and colour. Excess of this
ingredient seriously affect the soundness of cement.
Alkalies in excess are disadvantageous as they may cause alkali aggregate reaction,
efflorescence and staining of concrete and brickwork. Generally alkalies present in the raw
materials get removed by the flue gases in the burning process.

Harmful ingredients in cement:


i. Excess of Alumina reduces the strength.
ii. Magnesia content should not exceed 8%. This will affect soundness of cement.
iii. Excess of lime produces objectionable expansion leading to disintegration.
iv. Excess of alkalies produces alkali aggregate reaction, efflorescence.

Manufacturing of cement:
The three distinct operations involved in the manufacture of cement are:\
(i) Mixing of raw materials.
(ii) Burning.
(iii) Grinding.
Mixing of raw materials: The raw materials of cement are lime stone and clay are mixed in
dry condition or wet condition. Accordingly the process of mixing is called dry process or wet
process.
Dry process: This is an outdated process. In this process lime stone and clay are broken into
pieces of nearly 25 mm size by crushers. An air draft is passed over the crushed materials.
Now these are ground to a fine powder in the grinding mills. Each ingredient is separately
stored in separate hoppers.
The powdered materials are now mixed in the required proportion. The raw mix so obtained
is stored in the storage tank. From the storage tank the raw mix is passed on to the
granulator consisting to a sloping rotating drum. Water about 15% is sprinkled and powdered
material to become nodules. These are now burnt in the kiln.
Wet process: The raw materials viz. limestone and clay are taken in the right proportion and
crushed to a fine powder in jaw crushers. The crushed materials in the proper proportionare
conveyed into the ball mill. Water is added and the mixture is ground to form a slurry. The
slurry is conveyed into the correcting silos in which the chemical composition of the slurry is
examined. Now the slurry is passed on to the rotary kiln.
Burning: The slurry is burnt in a rotary kiln. The rotary kiln consists of a long cylinder 50 m to
100 m long supported on roller bearings provided over masonry pillars at intervals of 15 m to

Page no: 11 Follow us on facebook to get real-time updates from RGPV


Downloaded from be.rgpvnotes.in

Subject Name: Basic Civil Engineering & Engineering Mechanics Subject Code: BT-2004

20 m. The inner surface of the cylinder is lined with fire bricks. The cylinder is placed at a
slope of 1 in 30. The cylinder rotates at1 revolution per minute. The heating is done by
injecting pulverized coal using hot air blast from the lower end, while the slurry from hopper
is supplied at the upper end. The slurry soon changes into nodules which roll down the kiln
reaching hotter zones. As the nodules are heated to a very high temperature (1600°C), they
are changed into hard clinkers. The white hot clinkers discharged out of the kiln are cooled in
coolers by passing cold air.
Grinding: The clinkers are now ground in the ball mills and finally in the Tube mills. About 2%
to 4% of gypsum is added to control the setting time of cement. After completion of grinding
the cement is sieved and packed in bags.
Testing of Portland cement:
Field tests for cement:
When cement is received at a construction site, a few field tests can be made to ascertain its
quality. They are
1) Cement should be uniform in colour. Portland cement should be greenish grey in
colour.
2) When a small sample of cement is rubbed between fingers, it should feel smooth.
3) The cement mass must feel cool when touched by hand.
4) There should be no lumps in the cement. Lumps indicate cement that has already set.

Figure 4: The cement (left) and clinker (right)


Laboratory tests for cement: To ascertain the qualities of cement correctly, a number of tests
are performed in the laboratory as suggested by IS codes. They are;
1) Sampling: A sample meant for testing shall be drawn from at least 12 different bags or
barrels or containers or from 12 different positions in heap if the cement is loose. The
final sample shall weigh at least 5 kg. The sample is placed in a dry metal can closed
with tight cover to exclude external air and moisture.
2) Chemical Composition: The IS specified tests are;
i. Ignition loss: One gram of sample is heated in a porcelain crucible continuously
for a period of 1 hour at 900°C to 1000°C. If platinum crucible is used, it is
enough to heat the sample for 15 minutes. After heating the sample, it is
cooled and again weighed. The percentage loss of weight should not exceed
4%.
ii. Insoluble residue: one gram of cement is weighed and put in a 40 cc of water
and stirred. Then 10 cc of hydrochloric acid of specific gravity 1.18 should be

Page no: 12 Follow us on facebook to get real-time updates from RGPV


Downloaded from be.rgpvnotes.in

Subject Name: Basic Civil Engineering & Engineering Mechanics Subject Code: BT-2004

added and stirred. Any lumps present shall be carefully broken and the mixture
is boiled for 10 minutes. The mixture, now, shall be filtered. Using hot water
the container should be rinsed 5times and the filter should be washed 10
times. Now the residue left on the filter should be washed in a beaker
containing 30 cc of hot distilled water. This is boiled for a duration of 10
minutes with 30 cc of sodium carbonate solution of twice the normal strength.
The solution obtained is again filtered through the same filter paper. The filter
paper is now washed 5 times with water. Now it is washed with hydrochloric
acid solution of twice the normal strength and then with water so that it is free
from chlorides. The filter paper is dried, then ignited and weighed. The
insoluble residue shall not exceed 1.5%.
iii. Lime and alumina: The ratio of percentage alumina to the percentage of iron
oxide shall not be less than 0.66. The percentage of lime to silica. Alumina and
iron oxide when determined by the formula in percentage
(CaO – 0.7SO2) / (2.8Sio2 + 1.2 Al2O3 + 0.65Fe2O3)
Should not exceed 1.02 nor be less than 0.65.
iv. Magnesia: Free magnesia shall not be present at more than 5 percent.
v. Sulphur: This shall not exceed 2.75%.
3) Fineness: Sieve test: 100 grams of cement is weighed accurately and placed on IS sieve
No. 9. Any air set lumps are broken using fingers. Now gentle sieving is done
continuously for fifteen minutes. The residue left is weighed. This shall not exceed
10% by weight of the sample.
Air permeability test: In this test specific surface in square cm per gram of cement is
measured. The permissible values as given below:

Sl. Type of cement Specific surface area


No. requirement in
2
cm /gm
1 Ordinary Portland cement 2250
2 Portland blast furnace slag 2250
cement
3 Rapid hardening Portland cement 3250
4 Low heat Portland cement 3200
5 Portland pozzolana cement 3000

Page no: 13 Follow us on facebook to get real-time updates from RGPV


Downloaded from be.rgpvnotes.in

Subject Name: Basic Civil Engineering & Engineering Mechanics Subject Code: BT-2004

Figure 3: Vicat Apparatus with plunger and needle.

4) Consistency: This is a test conducted to estimate the quantity of water to be mixed


with cement to form a paste of normal consistency for use in other tests. 300 grams of
cement is mixed with 25% of water and a paste is prepared. The paste obtained
should e filled i the ould of the Vi at’s apparatus. The i ter al of ti e et ee
the instant of adding water to the dry cement and the instant of common cement of
filling the mould is called the time of gauging. The time of gauging must be 4±0.25
minutes.
The plunger, of diameter 10 mm is lowered gently on the paste in the mould. Now the
settlement of plunger is noted. If the settlement is between 5 and 7 mm from the
bottom of the mould, the amount of water added is correct. If this condition is not
satisfied, the test must be repeated again by changing the percentage of water until
the stipulated extent of penetration of the plunger is reached.

5) Test for setting time: The object of this test is to make a distinction between normal
setting and quick setting types of cement and also to detect deterioration due to
storage.
Weigh 300 grams of cement and add the percentage of water required to have normal
o siste . The paste o tai ed is filled i the ould. I the Vi at’s apparatus, atta h
the needle of square se tio i.e. to the Vi at’s rod. Lo er the s ste so
that the needle just touches the surface of the paste and gently release. Find out if the
needle pierces into the paste fully. If it does, again observe whether the needle
pierces fully into the paste. This is repeated till the needle does not pierce into the
paste completely. Now the interval of time between this instant and the instant at
which water was added to the cement is called the initial setting time.

Page no: 14 Follow us on facebook to get real-time updates from RGPV


Downloaded from be.rgpvnotes.in

Subject Name: Basic Civil Engineering & Engineering Mechanics Subject Code: BT-2004

Now change the needle to the third one which has a projecting sharp point in the
centre with an annular attachment. Now release the needle as before on the same
paste. The needle as well as the attachment will make their impressions on the paste.
Repeat this process till only the needle makes the impression but not the attachment.
The interval of time between this instant and the instant at which water was added to
the cement is called the final setting time.

Figure 4: Le Chatelier apparatus


6) Test for Soundness: If excess of lime is present during the manufacture of cement, it is
liable to remain uncombined and over burnt in the kiln. Such over burnt lime particles
slake at very slow rate and expand. If after setting of cement is completed, the over
burnt lime expand, it will lead to the disruption of cement mass. The object of the
soundness test is to detect the presence of over-burnt uncombined lime. The cement
is tested by using Le Chatelier apparatus as shown in Figure 4.
This apparatus consists of a small split cylinder of brass 0.5 mm thick. This forms a
mould 30 mm internal diameter and 30 mm in height. On each side of the split an
indicator is attached having pointed end. The distance between the centre of cylinder
and the pointed end of each indicator is 165 mm. The mould is placed on a glass plate
and is then filled with cement paste. The cement paste should be formed by gauging
with 0.78 of the water required to give a paste of normal consistency. After filling the
mould, another glass plate is placed on the top and is immediately submerged in
water at a temperature of 27°C to 32°C for 24 hours. After this interval of time, the
distance between the ends of the pointers is measured. Now the mould is again
submerged and brought to boiling point in 25 to 30 minutes and boiled for duration of
one hour. Then the mould is taken out of water and the distance between the ends of
the pointers is measured. The difference between this measurement and the original
measurement should not exceed 10 mm.
7) Tensile strength: The tensile strength of cement is estimated by determining the
tensile strength of cement sand mortar. For conducting the test briquettes of standard
size are prepared. The briquettes are 2.54 cm thick and will have a minimum sectional
area 2.54 cm x 2.54 cm. The cement mortar is made by mixing one part of cement to

Page no: 15 Follow us on facebook to get real-time updates from RGPV


Downloaded from be.rgpvnotes.in

Subject Name: Basic Civil Engineering & Engineering Mechanics Subject Code: BT-2004

three parts of Leighton Buzzard sand. The percentage of water to be used for making
the mix is 0.2Pa + 2.5 where Pa is the percentage of water for normal consistency of
cement. At least 12 briquettes are to be made. After the mould is made a small heap
of paste is placed on the top and is lightly beaten with the standard spatula until on
the surface water appears. Now the same is repeated on the other face of the
briquette. The briquettes are kept in a damp tank, the relative humidity in the tank
being 90%. Now six briquettes are tested after 3 days and the other six after 7 days in
a testing machine to destruction. The load must be increased at the rate of 3.5 N/mm 2
of section for each minute.
Stress at failure = Load at failure/Minimum sectional area of briquette.
The following are the requirements for good cement.

Sl. Type of cement Tensile strength in N/mm2.


No.
1 Portland cement 3 days Not less than 2.0 7 days Not less than 2.5
2 Rapid hardening cement 1 days Not less than 2.0 3 days Not less than 3.0

8) Compressive strength: This is a test to study the quality of cement about compressive
strength. The compressive strength is studied by determining the compressive
strength of cement sand mortar.
180 grams of cement should be mixed with 3 times its weight of standard Leighton
Buzzard sand for one minute and then mixed with water whose percentage is given by
P = (Pa/4) + 3.5
where Pa is the percentage of water for normal consistency. The mixing should be
done for 3 minutes. And in this duration the mixture must reach a uniform color. The
mould shall be of 7.06 cm side. The mortar is filled in the mould and the compaction is
done by using a standard vibration machine for 2 minutes. After this the cubes are
kept at a temperature for about 27°C in a chamber for 24 hours in which the relative
humidity is 90%. After this the cubes are removed from the moulds and are kept
under fresh water till they are tested.
3 cubes are tested at the end of three days and 3 more may be tested at the end of 7
days. The strength requirements are given below.
After 3 days: 11.5 N/mm2 for ordinary cement.
21.0 N/mm2 for Rapid hardening cement.
After 7 days: 17.5 N/mm2 for ordinary cement.

Page no: 16 Follow us on facebook to get real-time updates from RGPV


We hope you find these notes useful.
You can get previous year question papers at
https://qp.rgpvnotes.in .

If you have any queries or you want to submit your


study notes please write us at
rgpvnotes.in@gmail.com

You might also like