R. Guehne robin.guehne@cpfs.mpg.de    J. Noky    C. Yi    C. Shekhar Max Planck Institute for Chemical Physics of Solids, 01187, Dresden, Germany    M. G. Vergniory Max Planck Institute for Chemical Physics of Solids, 01187, Dresden, Germany Donostia International Physics Center, 20018 Donostia - San Sebastian, Spain    M. Baenitz    C. Felser Max Planck Institute for Chemical Physics of Solids, 01187, Dresden, Germany
Abstract

The Kagome network is a unique platform in solid state physics that harbors a diversity of special electronic states due to its inherent band structure features comprising Dirac cones, van-Hove singularities, and flat bands. Some Kagome-based non-magnetic metals have recently been found to exhibit favorable properties, including unconventional superconductivity, charge density waves (CDW), switchable chiral transport, and signatures of an anomalous Hall effect (AHE). The Kagome metal ScV6Sn6 is another promising candidate for studying the emergence of an unconventional CDW and accompanying effects. We use 51V nuclear magnetic resonance (NMR) to study the local properties of the CDW phase in single crystalline ScV6Sn6, aided by density functional theory (DFT). We trace the dynamics of the local magnetic field during the CDW phase transition and determine a loss in the density of states (DOS) by a factor of 22\sqrt{2}square-root start_ARG 2 end_ARG, in excellent agreement with DFT. The local charge symmetry of the V surrounding in the CDW phase reflects the commensurate modulation of the charge density with wave vector q=(13,13,13)π‘ž131313q=\left(\frac{1}{3},\frac{1}{3},\frac{1}{3}\right)italic_q = ( divide start_ARG 1 end_ARG start_ARG 3 end_ARG , divide start_ARG 1 end_ARG start_ARG 3 end_ARG , divide start_ARG 1 end_ARG start_ARG 3 end_ARG ). An unusual orientation dependent change in the NMR shift splitting symmetry, however, reveals orbital selective modulations of the local DOS.

Kagome lattice, charge density wave, nuclear magnetic resonance

Introduction

Covalent two-dimensional metals with triangular motifs and confined electronic states are a rich playground in modern solid states physics. Among the non-magnetic materials, systems that are based on Kagome layers attract increasing attention as they naturally feature Dirac cones, van-Hove singularities, and flat bands in their electronic band structure, that may further chemically be tuned to the vicinity of the Fermi level [1]. Lately, the V based Kagome metal CsV3Sb5 appeared in the spotlight as it undergoes a charge density wave (CDW) phase transition around 94Β Ktimes94K94\text{\,}\mathrm{K}start_ARG 94 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG before it becomes an unconventional superconductor below about 2Β Ktimes2K2\text{\,}\mathrm{K}start_ARG 2 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG, providing the prospect to learn more about the interplay of both phenomena. Evidence for a manipulable chiral transport as well as an anomalous Hall effect (AHE) in the CDW regime further add to the rather diverse list of special electronics of this Kagome metal [2, 3].

Recently, the closely related bilayer Kagome material ScV6Sn6 was reported to undergo a CDW transition at about 92Β Ktimes92K92\text{\,}\mathrm{K}start_ARG 92 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG, including evidence for topologically non-trivial bands and signatures of an anomalous Hall effect, while superconductivity was not observed at ambient pressure [4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24]. In particular the unconventional nature of CDW phase with a 3-dimensional wavevector πͺ3=(13,13,13)subscriptπͺ3131313\mathbf{q}_{3}=\left(\frac{1}{3},\frac{1}{3},\frac{1}{3}\right)bold_q start_POSTSUBSCRIPT 3 end_POSTSUBSCRIPT = ( divide start_ARG 1 end_ARG start_ARG 3 end_ARG , divide start_ARG 1 end_ARG start_ARG 3 end_ARG , divide start_ARG 1 end_ARG start_ARG 3 end_ARG ) gives rise to an ongoing debate about the formation mechanism of the charge order [5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 16, 17, 18, 19, 20, 21]. Some experiments and theory further suggest a high temperature short range CDW with πͺ2=(13,13,12)subscriptπͺ2131312\mathbf{q}_{2}=\left(\frac{1}{3},\frac{1}{3},\frac{1}{2}\right)bold_q start_POSTSUBSCRIPT 2 end_POSTSUBSCRIPT = ( divide start_ARG 1 end_ARG start_ARG 3 end_ARG , divide start_ARG 1 end_ARG start_ARG 3 end_ARG , divide start_ARG 1 end_ARG start_ARG 2 end_ARG ) that is unstable at low temperatures [9, 10, 11, 13, 21].

The complexity of the CDW as well as numerous experimental reports of unusual phenomena led us to employ nuclear magnetic resonance (NMR) to characterize the CDW phase of single crystalline ScV6Sn6 and to search for signatures of an unusual magnetism. Given its high sensitivity for chemical and electronic properties, as well as the atomic resolution, NMR has a long tradition as a method to investigate charge ordered systems, as e.g., in the case of the famous dichalcogenides [25]. In the context of cuprates, NMR is used to deepen the understanding of the interplay between charge order and superconductivity [26, 27]. Similarly, NMR of CsV3Sb5 has led to crucial insights into the charge modulation at ambient and elevated pressure [28, 29, 30, 31, 1].

With this paper we present a comprehensive single crystal 51V NMR study of the Kagome metal ScV6Sn6 aided by density functional theory (DFT). We explore the dynamic properties of the local magnetic field during the CDW phase transition between 96Β times96absent96\text{\,}start_ARG 96 end_ARG start_ARG times end_ARG start_ARG end_ARG and about 80Β Ktimes80K80\text{\,}\mathrm{K}start_ARG 80 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG, and determine a drop in the density of states (DOS) by a factor of 22\sqrt{2}square-root start_ARG 2 end_ARG. The CDW phase is characterized as a commensurate, threefold modulation of the local V charge symmetry in accordance with the reported reconstruction of the unit cell with periodicity 3Γ—3Γ—3333\sqrt{3}\times\sqrt{3}\times 3square-root start_ARG 3 end_ARG Γ— square-root start_ARG 3 end_ARG Γ— 3. Our NMR shift data further reveal a peculiar phase shift Δ⁒φ=Ο€/2Ξ”πœ‘πœ‹2\Delta\varphi=\pi/2roman_Ξ” italic_Ο† = italic_Ο€ / 2 of the sinusoidal modulation of the local magnetic field between the in-plane and the out-of-plane field orientation. This observation can be explained by orbital selective modulations of the local DOS resulting in a distinct wave vector for the V 3dz2subscript𝑑superscript𝑧2d_{z^{2}}italic_d start_POSTSUBSCRIPT italic_z start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT end_POSTSUBSCRIPT orbitals with qz2=(13,13,23)subscriptπ‘žsuperscript𝑧2131323q_{z^{2}}=\left(\frac{1}{3},\frac{1}{3},\frac{2}{3}\right)italic_q start_POSTSUBSCRIPT italic_z start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT end_POSTSUBSCRIPT = ( divide start_ARG 1 end_ARG start_ARG 3 end_ARG , divide start_ARG 1 end_ARG start_ARG 3 end_ARG , divide start_ARG 2 end_ARG start_ARG 3 end_ARG ). Finally, we neither find direct evidence of an unusual magnetism as related to time-reversal symmetry breaking and an AHE, nor of an additional, high temperature charge modulation with πͺ2=(13,13,12)subscriptπͺ2131312\mathbf{q}_{2}=\left(\frac{1}{3},\frac{1}{3},\frac{1}{2}\right)bold_q start_POSTSUBSCRIPT 2 end_POSTSUBSCRIPT = ( divide start_ARG 1 end_ARG start_ARG 3 end_ARG , divide start_ARG 1 end_ARG start_ARG 3 end_ARG , divide start_ARG 1 end_ARG start_ARG 2 end_ARG ).

Refer to caption
Figure 1: One-dimensional commensurate CDWs and NMR (A) A chain of equidistant atoms with evenly distributed electron density (gray circles) yields a single NMR signal at K0subscript𝐾0K_{0}italic_K start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT (including intrinsic broadening). (B) For a CDW of amplitude Ξ΄β’Οπ›ΏπœŒ\delta\rhoitalic_Ξ΄ italic_ρ, periodicity q=1/2π‘ž12q=1/2italic_q = 1 / 2, and phase Ο†=0πœ‘0\varphi=0italic_Ο† = 0, local charge density peaks and valleys alternate between neighboring atoms, yielding a symmetric splitting into two resonance lines at ±δ⁒K∝δ⁒ρproportional-toplus-or-minusπ›ΏπΎπ›ΏπœŒ\pm\delta K\propto\delta\rhoΒ± italic_Ξ΄ italic_K ∝ italic_Ξ΄ italic_ρ. The signal intensity is proportional to the number of nuclei with the same local environment. (C) A CDW with q=1/3π‘ž13q=1/3italic_q = 1 / 3 yields 3 equally intense resonance lines. For Ο†=Ο€/2πœ‘πœ‹2\varphi=\pi/2italic_Ο† = italic_Ο€ / 2, two of them are symmetrically shifted to higher and lower frequencies, while the third one remains un-shifted (no extra charge). (D) For the special case of Ο†=Ο€πœ‘πœ‹\varphi=\piitalic_Ο† = italic_Ο€, two of the 3 lines overlap at δ⁒K/2𝛿𝐾2\delta K/2italic_Ξ΄ italic_K / 2, while the third one is shifted by δ⁒K𝛿𝐾\delta Kitalic_Ξ΄ italic_K in the opposite direction.

Charge density waves and NMR In the 1960s, Overhauser considered a sinusiodal modulation of the local spin and charge density in metals which is translated into characteristic spectral changes of the corresponding NMR signal through the variation in the NMR shift or quadrupole interaction (as will be discussed in more detail below) [32]. Consider a one-dimensional (1D) sinusiodal modulation of the local electronic density with wavelength Ξ»=2⁒π/qπœ†2πœ‹π‘ž\lambda=2\pi/qitalic_Ξ» = 2 italic_Ο€ / italic_q,

ρ=ρ0+δ⁒ρ⁒cos⁑(qβ‹…x+Ο†).𝜌subscript𝜌0π›ΏπœŒβ‹…π‘žπ‘₯πœ‘\rho=\rho_{0}+\delta\rho\cos(q\cdot x+\varphi)\ .italic_ρ = italic_ρ start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT + italic_Ξ΄ italic_ρ roman_cos ( italic_q β‹… italic_x + italic_Ο† ) . (1)

Here, ρ0subscript𝜌0\rho_{0}italic_ρ start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT denotes the average or un-modulated charge in the CDW regime, Ξ΄β’Οπ›ΏπœŒ\delta\rhoitalic_Ξ΄ italic_ρ the amplitude, qπ‘žqitalic_q the wave vector, xπ‘₯xitalic_x the real-space position, and Ο†πœ‘\varphiitalic_Ο† the phase of the CDW. That is, different to most other methods, NMR can also determine the phase Ο†πœ‘\varphiitalic_Ο† of a charge modulation which can be an important detail in terms of the dynamics of CDWs [33]. A variety of commensurate CDW scenarios beside the corresponding NMR signals are illustrated in Fig.Β 1. We assume a periodic lattice of atoms with lattice parameter aπ‘Žaitalic_a and a uniform local electron density ρ0subscript𝜌0\rho_{0}italic_ρ start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT (panel A). The NMR signal appears at a K0subscript𝐾0K_{0}italic_K start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT that corresponds to the uniform local charge. In panels (B) to (D) of Fig.Β 1 we show three different CDWs and their NMR resonance patterns. The charge density variation is represented by the size of the circles. The NMR line splits with a maximum of 2⁒δ⁒K∝δ⁒ρproportional-to2π›ΏπΎπ›ΏπœŒ2\delta K\propto\delta\rho2 italic_Ξ΄ italic_K ∝ italic_Ξ΄ italic_ρ. Here, NMR shifts to higher and lower frequencies display the gain or loss of electron density for the respective crystal position. In general, the sign of δ⁒K𝛿𝐾\delta Kitalic_Ξ΄ italic_K does not allow a conclusion on whether the corresponding nucleus sits in a valley or on a peak of the CDW, as it depends on the type of hyperfine interaction [34]. For q=1/2π‘ž12q=1/2italic_q = 1 / 2 (as for 51V NMR in CsV3Sb5), the resonance line always splits symmetrically, independent of the CDW phase. Contrastingly, for q=1/3π‘ž13q=1/3italic_q = 1 / 3, as in case of 51V NMR of ScV6Sn6, the relative position of the three resonances depends on Ο†πœ‘\varphiitalic_Ο† (cf. panels C and D). This simple model is easily extended to incommensurate CDWs that give rise to broadened NMR spectra with a characteristic double-peak structure at ±δ⁒Kplus-or-minus𝛿𝐾\pm\delta KΒ± italic_Ξ΄ italic_K.[32, 27]

Refer to caption
Figure 2: The crystal structures of ScV6Sn6 (A) On the left, side view of the high temperature unit cell of ScV6Sn6, and below, top view of the V Kagome lattice (red). In the CDW phase, the relative position of the Sn-Sc-Sn chains (gray and purple) is altered along the crystal c𝑐citalic_c-axis, yielding 3 different Sc-Sn-Sc units as depicted in panel (B) containing one V Kagome double layer each. This expands the unit cell by a factor of three. The displacement affects the distance of the Kagome-close Sn atoms (1,2,3), creating 3 distinct V crystal sites (V1, V2, V3).

The structural phases of ScV6Sn6 The high temperature phase of ScV6Sn6 has P6/mmm symmetry. The unit cell consists of 13 atoms, where chemically equivalent Vanadium atoms form the Kagome planes, cf. Fig.Β 2Β (A). Below about 96Β Ktimes96K96\text{\,}\mathrm{K}start_ARG 96 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG, ScV6Sn6 undergoes a structural phase transition yielding a change in the Sc and Sn positions along the crystal c𝑐citalic_c-axis, while the V lattice remains almost unperturbedΒ [5]. In panel (B) of Fig.Β 2, we show the relevant displacements in terms of Sn-Sc-Sn chains (gray-purple-gray) containing two Kagome layers (red). Different to the symmetric arrangement characteristic for the high T𝑇Titalic_T phase, the low T𝑇Titalic_T phase features 3 Sn-Sc-Sn chains that vary in length and in relative distance to the V Kagome plane. From the viewpoint of the V Kagome lattice, we identify 3 corresponding Sn positions (1, 2, 3) that hover just above (below) the hexagonal V voids, creating 3 non-equivalent V crystal sites (V1, V2, V3), each of them neighbored by two different Sn sites as shown in the lower panel of Fig.Β 2 (B).

Refer to caption
Figure 3: The local Vanadium charge symmetry for high and low temperatures (A) The Fourier transform of the 51V NMR spectra (from selective spin echoes) for 8.73Β Ttimes8.73T8.73\text{\,}\mathrm{T}start_ARG 8.73 end_ARG start_ARG times end_ARG start_ARG roman_T end_ARG and cβˆ₯B0conditional𝑐subscript𝐡0c\parallel B_{0}italic_c βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT. The spectra were obtained at 110Β times110absent110\text{\,}start_ARG 110 end_ARG start_ARG times end_ARG start_ARG end_ARG and 80Β Ktimes80K80\text{\,}\mathrm{K}start_ARG 80 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG, confronting the spectral differences between the high and the low temperature phase. The central frequency has been subtracted for the clarity. (B) High temperature orientation dependent quadrupole splittings for rotations about the crystal c𝑐citalic_c-axis (in-plane) reveals the six-fold rotation symmetry of the Kagome lattice (cf. Fig.Β 9). Perspective view (C) and top view (D) of the equivalent EFGs at V sites in the Kagome lattice. (E) Low temperature orientation dependent quadrupole splittings for in-plane rotations confirms the three sets of quadrupole patterns already observed in panel (A), while the six-fold rotation symmetry of the Kagome lattice is conserved (cf. Fig.Β 11). (F) Thus, for low temperatures, the three corners of each V triangle become chemically non-equivalent while the EFGs keep the orientation of the high T𝑇Titalic_T phase. (G) The commensurate variation of the EFGs along the crystal aπ‘Žaitalic_a or b𝑏bitalic_b axis, can be viewed as a 1D sinusoidal modulation with q=1/3π‘ž13q=1/3italic_q = 1 / 3 and Ο†β‰ˆΟ€/4πœ‘πœ‹4\varphi\approx\pi/4italic_Ο† β‰ˆ italic_Ο€ / 4.

Results

The local Vanadium charge symmetry The above discussed structural phases feature different local V environments. NMR allows to differentiate them via the electric quadrupole interaction, if such environments have non-cubic symmetry and the nuclear spin satisfies I>1/2𝐼12I>1/2italic_I > 1 / 2 (I51=7/2superscript𝐼5172{}^{51}I=7/2start_FLOATSUPERSCRIPT 51 end_FLOATSUPERSCRIPT italic_I = 7 / 2). In first order approximation, the quadrupole interaction can be written as

β„‹Qsubscriptβ„‹Q\displaystyle\mathcal{H}_{\mathrm{Q}}caligraphic_H start_POSTSUBSCRIPT roman_Q end_POSTSUBSCRIPT =3⁒Iz2βˆ’I⁒(I+1)4⁒I⁒(2⁒Iβˆ’1)⁒e⁒Q⁒VZ⁒Zabsent3superscriptsubscript𝐼𝑧2𝐼𝐼14𝐼2𝐼1𝑒𝑄subscript𝑉𝑍𝑍\displaystyle=\frac{3I_{z}^{2}-I(I+1)}{4I(2I-1)}eQV_{ZZ}= divide start_ARG 3 italic_I start_POSTSUBSCRIPT italic_z end_POSTSUBSCRIPT start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT - italic_I ( italic_I + 1 ) end_ARG start_ARG 4 italic_I ( 2 italic_I - 1 ) end_ARG italic_e italic_Q italic_V start_POSTSUBSCRIPT italic_Z italic_Z end_POSTSUBSCRIPT (2)
Γ—12⁒(3⁒cos2β‘Ξ²βˆ’1+η⁒sin2⁑β⁒cos⁑α),absent123superscript2𝛽1πœ‚superscript2𝛽𝛼\displaystyle\times\frac{1}{2}\left(3\cos^{2}\beta-1+\eta\sin^{2}\beta\cos% \alpha\right)\ ,Γ— divide start_ARG 1 end_ARG start_ARG 2 end_ARG ( 3 roman_cos start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT italic_Ξ² - 1 + italic_Ξ· roman_sin start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT italic_Ξ² roman_cos italic_Ξ± ) ,

where e⁒Q𝑒𝑄eQitalic_e italic_Q is the nuclear quadrupole moment and VZ⁒Zsubscript𝑉𝑍𝑍V_{ZZ}italic_V start_POSTSUBSCRIPT italic_Z italic_Z end_POSTSUBSCRIPT is the principle value of the electric field gradient (EFG). The EFG is derived from the charge distribution at the nucleus’ position, and is thus tightly connected to the above mentioned local environment. The EFG is represented as a traceless (VZ⁒Z+VY⁒Y+VX⁒X=0subscript𝑉𝑍𝑍subscriptπ‘‰π‘Œπ‘Œsubscript𝑉𝑋𝑋0V_{ZZ}+V_{YY}+V_{XX}=0italic_V start_POSTSUBSCRIPT italic_Z italic_Z end_POSTSUBSCRIPT + italic_V start_POSTSUBSCRIPT italic_Y italic_Y end_POSTSUBSCRIPT + italic_V start_POSTSUBSCRIPT italic_X italic_X end_POSTSUBSCRIPT = 0), second rank tensor. It is conveniently expressed in terms of its size (|VZ⁒Z|subscript𝑉𝑍𝑍|V_{ZZ}|| italic_V start_POSTSUBSCRIPT italic_Z italic_Z end_POSTSUBSCRIPT |) and shape given by the asymmetry parameter Ξ·=(VX⁒Xβˆ’VY⁒Y)/VZ⁒Zπœ‚subscript𝑉𝑋𝑋subscriptπ‘‰π‘Œπ‘Œsubscript𝑉𝑍𝑍\eta=(V_{XX}-V_{YY})/V_{ZZ}italic_Ξ· = ( italic_V start_POSTSUBSCRIPT italic_X italic_X end_POSTSUBSCRIPT - italic_V start_POSTSUBSCRIPT italic_Y italic_Y end_POSTSUBSCRIPT ) / italic_V start_POSTSUBSCRIPT italic_Z italic_Z end_POSTSUBSCRIPT (|VZ⁒Z|β‰₯|VY⁒Y|β‰₯|VX⁒X|subscript𝑉𝑍𝑍subscriptπ‘‰π‘Œπ‘Œsubscript𝑉𝑋𝑋|V_{ZZ}|\geq|V_{YY}|\geq|V_{XX}|| italic_V start_POSTSUBSCRIPT italic_Z italic_Z end_POSTSUBSCRIPT | β‰₯ | italic_V start_POSTSUBSCRIPT italic_Y italic_Y end_POSTSUBSCRIPT | β‰₯ | italic_V start_POSTSUBSCRIPT italic_X italic_X end_POSTSUBSCRIPT |). The Euler angles α𝛼\alphaitalic_Ξ± and β𝛽\betaitalic_Ξ² determine the relative orientation of the EFG’s principle axis system with respect to the external magnetic field (typically laboratory z𝑧zitalic_z-axis), and thus with respect to the sample’s crystal lattice.

From (2) it follows that the V nuclear spin system splits into 2⁒I=72𝐼72I=72 italic_I = 7 equidistant resonance lines (note, second order shifts amount to about 1Β kHztimes1kHz1\text{\,}\mathrm{k}\mathrm{H}\mathrm{z}start_ARG 1 end_ARG start_ARG times end_ARG start_ARG roman_kHz end_ARG in maximum), 1Β central transition (CT) and 3 pairs of satellites, as shown in the top spectrum of Fig.Β 3Β (A). The anisotropy of the interaction (α𝛼\alphaitalic_Ξ± and β𝛽\betaitalic_Ξ²) is transferred to the apparent quadrupolar line splitting Ξ½~Qsubscript~πœˆπ‘„\tilde{\nu}_{Q}over~ start_ARG italic_Ξ½ end_ARG start_POSTSUBSCRIPT italic_Q end_POSTSUBSCRIPT, i.e., the splitting depends on the sample orientation in the external field, as

Ξ½~Q=3⁒e⁒Q⁒VZ⁒Z4⁒I⁒(2⁒Iβˆ’1)⁒(3⁒cos2β‘Ξ²βˆ’1+η⁒sin2⁑β⁒cos⁑α),subscript~πœˆπ‘„3𝑒𝑄subscript𝑉𝑍𝑍4𝐼2𝐼13superscript2𝛽1πœ‚superscript2𝛽𝛼\tilde{\nu}_{Q}=\frac{3eQV_{ZZ}}{4I(2I-1)}\left(3\cos^{2}\beta-1+\eta\sin^{2}% \beta\cos\alpha\right)\ ,over~ start_ARG italic_Ξ½ end_ARG start_POSTSUBSCRIPT italic_Q end_POSTSUBSCRIPT = divide start_ARG 3 italic_e italic_Q italic_V start_POSTSUBSCRIPT italic_Z italic_Z end_POSTSUBSCRIPT end_ARG start_ARG 4 italic_I ( 2 italic_I - 1 ) end_ARG ( 3 roman_cos start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT italic_Ξ² - 1 + italic_Ξ· roman_sin start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT italic_Ξ² roman_cos italic_Ξ± ) , (3)

with the quadrupole splitting frequency defined as

Ξ½Q=3⁒e⁒Q⁒VZ⁒Z2⁒I⁒(2⁒Iβˆ’1).subscriptπœˆπ‘„3𝑒𝑄subscript𝑉𝑍𝑍2𝐼2𝐼1\nu_{Q}=\frac{3eQV_{ZZ}}{2I(2I-1)}\ .italic_Ξ½ start_POSTSUBSCRIPT italic_Q end_POSTSUBSCRIPT = divide start_ARG 3 italic_e italic_Q italic_V start_POSTSUBSCRIPT italic_Z italic_Z end_POSTSUBSCRIPT end_ARG start_ARG 2 italic_I ( 2 italic_I - 1 ) end_ARG . (4)

By evaluating Ξ½~Qsubscript~πœˆπ‘„\tilde{\nu}_{Q}over~ start_ARG italic_Ξ½ end_ARG start_POSTSUBSCRIPT italic_Q end_POSTSUBSCRIPT for various crystal orientations, size (|VZ⁒Z|subscript𝑉𝑍𝑍|V_{ZZ}|| italic_V start_POSTSUBSCRIPT italic_Z italic_Z end_POSTSUBSCRIPT |), shape (Ξ·πœ‚\etaitalic_Ξ·), and orientation of the EFG can be determined. In Fig.Β 3 (B) we show an example of this procedure for the high temperature phase (a detailed account is provided in the supplementary information SI), which corresponds to Ξ½~Q⁒(Ξ²,Ξ±=0)subscript~πœˆπ‘„π›½π›Ό0\tilde{\nu}_{Q}(\beta,\alpha=0)over~ start_ARG italic_Ξ½ end_ARG start_POSTSUBSCRIPT italic_Q end_POSTSUBSCRIPT ( italic_Ξ² , italic_Ξ± = 0 ), i.e., orientation dependent measurements under crystal rotation about the c𝑐citalic_c-axis (cf. Fig.Β 9 in SI). We find that VZ⁒Zsubscript𝑉𝑍𝑍V_{ZZ}italic_V start_POSTSUBSCRIPT italic_Z italic_Z end_POSTSUBSCRIPT points along to the crystal aβˆ—superscriptπ‘Žβˆ—a^{\ast}italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT-axis with Ξ½Q=475⁒(2)Β kHzsubscriptπœˆπ‘„timesuncertain4752kHz\nu_{Q}=$475(2)\text{\,}\mathrm{k}\mathrm{H}\mathrm{z}$italic_Ξ½ start_POSTSUBSCRIPT italic_Q end_POSTSUBSCRIPT = start_ARG start_ARG 475 end_ARG start_ARG ( 2 ) end_ARG end_ARG start_ARG times end_ARG start_ARG roman_kHz end_ARG and Ξ·=0.83⁒(1)Β πœ‚timesuncertain0.831absent\eta=$0.83(1)\text{\,}$italic_Ξ· = start_ARG start_ARG 0.83 end_ARG start_ARG ( 1 ) end_ARG end_ARG start_ARG times end_ARG start_ARG end_ARG. The three identical data sets (triangles, squares, and circles) shifted by Β±60Β Β°plus-or-minustimes60degree\pm$60\text{\,}\mathrm{\SIUnitSymbolDegree}$Β± start_ARG 60 end_ARG start_ARG times end_ARG start_ARG Β° end_ARG recover the six-fold symmetry of the Kagome lattice (insets) and prove the equivalency of the three corners of each V Kagome triangle in terms of the local Vanadium symmetry. To visualize the V EFGs in the Kagome lattice, we display them as ellipsoids formed by |VZ⁒Z|subscript𝑉𝑍𝑍|V_{ZZ}|| italic_V start_POSTSUBSCRIPT italic_Z italic_Z end_POSTSUBSCRIPT |, |VY⁒Y|subscriptπ‘‰π‘Œπ‘Œ|V_{YY}|| italic_V start_POSTSUBSCRIPT italic_Y italic_Y end_POSTSUBSCRIPT |, and |VX⁒X|subscript𝑉𝑋𝑋|V_{XX}|| italic_V start_POSTSUBSCRIPT italic_X italic_X end_POSTSUBSCRIPT |, as shown in panels (C) and (D) of Fig.Β 3.

Table 1: The electric quadrupole splitting frequency Ξ½Qsubscriptπœˆπ‘„\nu_{Q}italic_Ξ½ start_POSTSUBSCRIPT italic_Q end_POSTSUBSCRIPT, the principle axis of the electric field gradient VZ⁒Zsubscript𝑉𝑍𝑍V_{ZZ}italic_V start_POSTSUBSCRIPT italic_Z italic_Z end_POSTSUBSCRIPT from (3) (for the experiment, only the absolute value can be obtained, the sign cannot be accessed), and the asymmetry parameter Ξ·πœ‚\etaitalic_Ξ· as obtained from NMR and D⁒F⁒T𝐷𝐹𝑇DFTitalic_D italic_F italic_T at V positions above (High T𝑇Titalic_T) and below (Low T𝑇Titalic_T) the CDW phase transition.
High T𝑇Titalic_T Low T𝑇Titalic_T
NMR DFT NMR1 DFT1 NMR2 DFT2 NMR3 DFT3
Ξ½Qsubscriptπœˆπ‘„\nu_{Q}italic_Ξ½ start_POSTSUBSCRIPT italic_Q end_POSTSUBSCRIPT Β [kHz]timesabsentdelimited-[]kHz\text{\,}\mathrm{[}\mathrm{k}\mathrm{H}\mathrm{z}\mathrm{]}start_ARG end_ARG start_ARG times end_ARG start_ARG [ roman_kHz ] end_ARG 475(2) 463(2) 489(2) 499(2)
VZ⁒Zsubscript𝑉𝑍𝑍V_{ZZ}italic_V start_POSTSUBSCRIPT italic_Z italic_Z end_POSTSUBSCRIPT Β [1020⁒V/m2]timesabsentdelimited-[]superscript1020Vsuperscriptm2\text{\,}\mathrm{[}\mathrm{1}\mathrm{0}^{20}\mathrm{V}\mathrm{/}\mathrm{m}^{2}% \mathrm{]}start_ARG end_ARG start_ARG times end_ARG start_ARG [ 10 start_POSTSUPERSCRIPT 20 end_POSTSUPERSCRIPT roman_V / roman_m start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT ] end_ARG 52.9(2) -60.812 51.6(2) -59.679 54.4(2) -61.861 55.6(2) -62.617
Ξ·πœ‚\etaitalic_Ξ· 0.83(1) 0.809 0.91(4) 0.841 0.81(4) 0.782 0.78(3) 0.787

Upon cooling, between 96Β times96absent96\text{\,}start_ARG 96 end_ARG start_ARG times end_ARG start_ARG end_ARG and about 80Β Ktimes80K80\text{\,}\mathrm{K}start_ARG 80 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG, the phase transition takes place and the low temperature structure replaces the high T𝑇Titalic_T one. From the NMR point of view (Fig.Β 3 A lower spectrum), the changes are most prominently visible in a splitting of the low frequency satellites (find a detailed account on the temperature dependent spectra in Fig.Β 7 in the SI). The single quadrupole pattern observed for high temperature is replaced by 3 sets of quadrupole spectra. In panel (E) of Fig.Β 3 we show the results of the same orientation dependent measurements as in panel (B), now performed at 80Β Ktimes80K80\text{\,}\mathrm{K}start_ARG 80 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG (cf. Fig.Β 11 in SI). The change to a threefold quadrupole interaction is consistently found in any possible direction. This proves that the local Vanadium environments have changed, while the relative orientation of the 3 EFGs is same as at high temperatures. The arrangement of the EFGs is illustrated in panel (F). When viewed along the crystal aπ‘Žaitalic_a or b𝑏bitalic_b axis, panel (G), the 3 alternating EFGs create a commensurate 1D sinusoidal variation with q=1/3π‘ž13q=1/3italic_q = 1 / 3, Ο†=Ο€/4πœ‘πœ‹4\varphi=\pi/4italic_Ο† = italic_Ο€ / 4, and an amplitude of about 20Β kHztimes20kHz20\text{\,}\mathrm{k}\mathrm{H}\mathrm{z}start_ARG 20 end_ARG start_ARG times end_ARG start_ARG roman_kHz end_ARG around the average quadrupole splitting of 483.7Β kHztimes483.7kHz483.7\text{\,}\mathrm{k}\mathrm{H}\mathrm{z}start_ARG 483.7 end_ARG start_ARG times end_ARG start_ARG roman_kHz end_ARG. Detailed DFT calculations as implemented in VASPΒ [35, 36] confirm the results shown in Fig.Β 3, cf. Tab.1. Note that with the experiment we cannot determine the sign of VZ⁒Zsubscript𝑉𝑍𝑍V_{ZZ}italic_V start_POSTSUBSCRIPT italic_Z italic_Z end_POSTSUBSCRIPT since the quadrupole splitting is symmetric.

The CDW phase transition In Fig. 4 (A) we show the center line of the quadrupole spectra from Fig. 3 (A), for temperatures between 100 Ktimes100K100\text{\,}\mathrm{K}start_ARG 100 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG and 20 Ktimes20K20\text{\,}\mathrm{K}start_ARG 20 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG. For the sake of clarity, we have removed the (very small) temperature dependence of the NMR shift. At 96 Ktimes96K96\text{\,}\mathrm{K}start_ARG 96 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG, first indications of an additional signal (blue) appear about 15 kHztimes15kHz15\text{\,}\mathrm{k}\mathrm{H}\mathrm{z}start_ARG 15 end_ARG start_ARG times end_ARG start_ARG roman_kHz end_ARG (∼similar-to\sim∼150 ppmtimes150ppm150\text{\,}\mathrm{p}\mathrm{p}\mathrm{m}start_ARG 150 end_ARG start_ARG times end_ARG start_ARG roman_ppm end_ARG) next to the initial resonance line (gray). As this shoulder grows in intensity with decreasing temperature, the initial line decreases, until, for about 80 Ktimes80K80\text{\,}\mathrm{K}start_ARG 80 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG and below, the overall shape of the doublet remains unchanged.

In order to track the volume fractions of the two competing phases during the phase transition, we used Gaussian lines to fit the two resonances in panel (A) of Fig.Β 4 and extracted the corresponding signal intensities. The results are shown panel (B). The gray and blue data points denote the respective signal intensities of panel (A) (for an analysis of the total signal intensity, the reader is referred to Fig.Β 14 in the SI). The individual values are normalized with respect to their sum for each temperature. In the course of cooling, the low temperature resonance line (blue) grows to about 2/3 of the total intensity, leaving about 1/3 (gray) to what appears to be the initial high temperature line. With the colored dashed lines in Fig.Β 4 (B) we show the true changes in the relative intensities, concluded from the corresponding changes in the quadrupole splittings. The initial high temperature CT disappears entirely between 96 and about 80Β Ktimes80K80\text{\,}\mathrm{K}start_ARG 80 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG (black dashed line). It is replaced by three resonances (purple, orange, and light blue) with intensity ratio 1:1:1 that represent the 3 CTs of the low temperature quadrupole patterns identified in the former section. Two of the 3 resonances (orange and light blue) form the dark blue peak that appears during the phase transition in panel (A).

Refer to caption
Figure 4: CDW phase transition and the local magnetic field (A) The central region of the cβˆ₯B0conditional𝑐subscript𝐡0c\parallel B_{0}italic_c βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT spectrum as function of temperature at 8.73Β Ttimes8.73T8.73\text{\,}\mathrm{T}start_ARG 8.73 end_ARG start_ARG times end_ARG start_ARG roman_T end_ARG (Fourier transform of selective spin echoes). Highlighted is the temperature range of the phase transition. Gaussian lines (gray and blue) were used to fit the spectra and to extract the intensity changes. (B) The area of the Gaussians (proportional to signal intensity) from panel (A) as a function of temperature. Dashed lines denote true relative intensities. (C) and (D) The temperature dependence of the NMR shift for cβˆ₯B0conditional𝑐subscript𝐡0c\parallel B_{0}italic_c βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT and aβˆ—βˆ₯B0conditionalsuperscriptπ‘Žβˆ—subscript𝐡0a^{\ast}\parallel B_{0}italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT. Note that ”aβˆ—βˆ₯B0conditionalsuperscriptπ‘Žβˆ—subscript𝐡0a^{\ast}\parallel B_{0}italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT” holds only for 1 of the 3 V nuclei per V triangle as shown in the inset. Gray data points denote the average of the two and three low temperature shift values.

In Fig.Β 4Β (C) and (D) we show the temperature dependence of the NMR shift for the out-of-plane orientation of the magnetic field (cβˆ₯B0conditional𝑐subscript𝐡0c\parallel B_{0}italic_c βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT) and for the in-plane orientation (aβˆ—βˆ₯B0conditionalsuperscriptπ‘Žβˆ—subscript𝐡0a^{\ast}\parallel B_{0}italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT). In the latter case, a reliable determination of the shift values during the phase transition was not possible because of the overlap of high and low temperature resonance lines. For 80Β Ktimes80K80\text{\,}\mathrm{K}start_ARG 80 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG and below, the shift was determined via the satellite transitions (see SI). We assigned the shift values between cβˆ₯B0conditional𝑐subscript𝐡0c\parallel B_{0}italic_c βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT and aβˆ—βˆ₯B0conditionalsuperscriptπ‘Žβˆ—subscript𝐡0a^{\ast}\parallel B_{0}italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT as shown by the colors based on the DFT calculations. The assignment cannot be proven with experiment because the superposition of many resonance lines for orientation dependent measurements prevents a reliable tracing of individual signals. This, however, has no effect on the conclusions of the present investigation.

The V shift in ScV6Sn6 is with more than about 0.6Β %times0.6percent0.6\text{\,}\%start_ARG 0.6 end_ARG start_ARG times end_ARG start_ARG % end_ARG and 0.8Β %times0.8percent0.8\text{\,}\%start_ARG 0.8 end_ARG start_ARG times end_ARG start_ARG % end_ARG (6000Β ppmtimes6000ppm6000\text{\,}\mathrm{p}\mathrm{p}\mathrm{m}start_ARG 6000 end_ARG start_ARG times end_ARG start_ARG roman_ppm end_ARG to 8000Β ppmtimes8000ppm8000\text{\,}\mathrm{p}\mathrm{p}\mathrm{m}start_ARG 8000 end_ARG start_ARG times end_ARG start_ARG roman_ppm end_ARG) very large, strongly anisotropic, and only very weakly dependent on temperature (2 to 4Β %times4percent4\text{\,}\%start_ARG 4 end_ARG start_ARG times end_ARG start_ARG % end_ARG of the total shift). From detailed orientation dependent measurements (cf. Fig.Β 8 to 10 in the SI) it can be seen that the high temperature shift tensor is axially symmetric with the main axis pointing towards the center of the V triangle (along the aβˆ—superscriptπ‘Žβˆ—a^{\ast}italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT direction) similar to the EFG. Although it is very difficult to prove experimentally, it is reasonable to assume that the CDW phase inherits the axial shift anisotropy. Isotropic and axial shift components for the full range of temperatures are depicted in Fig.Β 13 in the SI.

Refer to caption
Figure 5: CDW phase transition and fluctuations of the local magnetic field (A) The spin-lattice relaxation rate 1/T11subscript𝑇11/T_{1}1 / italic_T start_POSTSUBSCRIPT 1 end_POSTSUBSCRIPT as a function of temperature obtained from the CT (cβˆ₯B0conditional𝑐subscript𝐡0c\parallel B_{0}italic_c βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT) for sample S1 and S2, and from the first low frequency satellite for aβˆ—βˆ₯B0conditionalsuperscriptπ‘Žβˆ—subscript𝐡0a^{\ast}\parallel B_{0}italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT. The inset shows the calculated DOS for V states at high (solid) and low (dashed line) temperatures. At EFsubscript𝐸FE_{\mathrm{F}}italic_E start_POSTSUBSCRIPT roman_F end_POSTSUBSCRIPT, the DOS drops by 22\sqrt{2}square-root start_ARG 2 end_ARG due to the CDW phase transition. (B) 1/T1⁒T1subscript𝑇1𝑇1/T_{1}T1 / italic_T start_POSTSUBSCRIPT 1 end_POSTSUBSCRIPT italic_T as a function of temperature. The blue solid line represents a fit for the high temperature phase data using (c⁒o⁒n⁒s⁒t.+T~TΓ—exp⁑(βˆ’Ξ”β’E/2kB⁒T))formulae-sequenceπ‘π‘œπ‘›π‘ π‘‘~𝑇𝑇Δ𝐸2subscriptπ‘˜π΅π‘‡\left(const.+\frac{\tilde{T}}{T}\times\exp\left(-\frac{\Delta E/2}{k_{B}T}% \right)\right)( italic_c italic_o italic_n italic_s italic_t . + divide start_ARG over~ start_ARG italic_T end_ARG end_ARG start_ARG italic_T end_ARG Γ— roman_exp ( - divide start_ARG roman_Ξ” italic_E / 2 end_ARG start_ARG italic_k start_POSTSUBSCRIPT italic_B end_POSTSUBSCRIPT italic_T end_ARG ) ) yielding T~∼730Β Ksimilar-to~𝑇times730K\tilde{T}\sim$730\text{\,}\mathrm{K}$over~ start_ARG italic_T end_ARG ∼ start_ARG 730 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG and Δ⁒E∼160Β meVsimilar-toΔ𝐸times160meV\Delta E\sim$160\text{\,}\mathrm{m}\mathrm{e}\mathrm{V}$roman_Ξ” italic_E ∼ start_ARG 160 end_ARG start_ARG times end_ARG start_ARG roman_meV end_ARG. Panel (C) shows the corresponding Arrhenius plot for the high temperature region above 150Β Ktimes150K150\text{\,}\mathrm{K}start_ARG 150 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG.

In panel (A) of Fig.Β 5 we show the spin-lattice relaxation rate of V nuclei in the two different samples, for two orientations (cβˆ₯B0conditional𝑐subscript𝐡0c\parallel B_{0}italic_c βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT and aβˆ—βˆ₯B0conditionalsuperscriptπ‘Žβˆ—subscript𝐡0a^{\ast}\parallel B_{0}italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT), and for a wide range of temperatures. After continuously decreasing between room temperature and about 100Β Ktimes100K100\text{\,}\mathrm{K}start_ARG 100 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG, 1/T11subscript𝑇11/T_{1}1 / italic_T start_POSTSUBSCRIPT 1 end_POSTSUBSCRIPT drops abruptly in the region of the phase transition by about a factor of 2. Between 80Β times80absent80\text{\,}start_ARG 80 end_ARG start_ARG times end_ARG start_ARG end_ARG and 4Β Ktimes4K4\text{\,}\mathrm{K}start_ARG 4 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG, the relaxation rate is proportional to the temperature. Measurements for aβˆ—βˆ₯B0conditionalsuperscriptπ‘Žβˆ—subscript𝐡0a^{\ast}\parallel B_{0}italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT (yellow circles) prove the spin-lattice relaxation to be isotropic (see also Fig.16 in the SI). In the low temperature phase, the data points represent the averaged relaxation of the 3 components. In the inset we present the Vanadium DOS for both phases obtained from DFT. The high temperature DOS are denoted by the solid line, the CDW phase DOS by the dashed line. At the Fermi level, the difference between high and low temperature DOS is 22\sqrt{2}square-root start_ARG 2 end_ARG, in agreement with the observed changes in the relaxation (cf. discussion). The temperature dependence of 1/T1⁒T1subscript𝑇1𝑇1/T_{1}T1 / italic_T start_POSTSUBSCRIPT 1 end_POSTSUBSCRIPT italic_T, as shown in panel (B), yields a constant value for temperatures below 80Β Ktimes80K80\text{\,}\mathrm{K}start_ARG 80 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG and a pronounced step during the phase transition. For temperatures above TCDWsubscript𝑇CDWT_{\mathrm{CDW}}italic_T start_POSTSUBSCRIPT roman_CDW end_POSTSUBSCRIPT and ≀150Β Kabsenttimes150K\leq$150\text{\,}\mathrm{K}$≀ start_ARG 150 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG, 1/T1⁒T1subscript𝑇1𝑇1/T_{1}T1 / italic_T start_POSTSUBSCRIPT 1 end_POSTSUBSCRIPT italic_T appears to be rather constant as well, while it clearly deviates from such a behavior for even higher temperatures. This progressive increase implies a gain in available states as, e.g., in the case of thermal excitation across an energy gap. An activation type of fit (blue line) gives a gap of about 160Β meVtimes160meV160\text{\,}\mathrm{m}\mathrm{e}\mathrm{V}start_ARG 160 end_ARG start_ARG times end_ARG start_ARG roman_meV end_ARG. In panel (C) we show the corresponding Arrhenius plot for the high temperature relaxation rate (above 150Β Ktimes150K150\text{\,}\mathrm{K}start_ARG 150 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG).

Discussion

General remarks The temperature dependent 51V spectra of ScV6Sn6 as shown in Fig.Β 3 (Fig.Β 7 in the SI) and 4 provide consistent evidence of a first order phase transition between 96Β times96absent96\text{\,}start_ARG 96 end_ARG start_ARG times end_ARG start_ARG end_ARG and about 80Β Ktimes80K80\text{\,}\mathrm{K}start_ARG 80 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG in good agreement with literature [15]. The low T𝑇Titalic_T phase is similarly homogeneous as the high T𝑇Titalic_T one, with no additional broadening, neither in the NMR shift nor in the quadrupole interaction, proving any observed changes in the static NMR at low temperatures are perfectly commensurate and sufficiently long range such that domain effects are negligible. Hence, our observations do not support the presence of an additional short-range intermediate charge order [9, 10, 11, 13, 21]. The results also do not provide any direct evidence of an unusual magnetism as related to TRS breaking and an anomalous Hall effect. The cβˆ₯B0conditional𝑐subscript𝐡0c\parallel B_{0}italic_c βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT-splitting in units of ppm as well as the line shape, i.e., the relative intensity of this double-peak structure, are independent of the applied magnetic field, and thus point at different local spin densities as expected for a CDW (cf. Fig.Β 15 in SI). Similarly, total signal intensity as well as excitation conditions of the NMR experiments do not indicate any effect from magnetism, as there are no unusual losses or enhancements. That is, any additional effect must be well below the observed linewidth of our resonance lines which is in the order of 100Β ppmtimes100ppm100\text{\,}\mathrm{p}\mathrm{p}\mathrm{m}start_ARG 100 end_ARG start_ARG times end_ARG start_ARG roman_ppm end_ARG.

Local properties of the CDW phase The EFG at V sites accessible through the V quadrupole interaction gives a direct evidence of a characteristic charge redistribution due to the CDW phase transition. As shown in the Fig.Β 3, the single high temperature Vanadium EFG is replaced by 3 low temperature EFGs differing in size and shape, but retaining the original orientation in the crystal lattice. The 3 different EFGs mapped on the known low temperature crystal structure correspond to a CDW with wave vector q=(13,13,13)π‘ž131313q=\left(\frac{1}{3},\frac{1}{3},\frac{1}{3}\right)italic_q = ( divide start_ARG 1 end_ARG start_ARG 3 end_ARG , divide start_ARG 1 end_ARG start_ARG 3 end_ARG , divide start_ARG 1 end_ARG start_ARG 3 end_ARG ) which agrees with the reported reconstruction of the unit cell with 3Γ—3Γ—3333\sqrt{3}\times\sqrt{3}\times 3square-root start_ARG 3 end_ARG Γ— square-root start_ARG 3 end_ARG Γ— 3 periodicity. From the splitting frequencies we determine the phase to be Ο†β‰ˆΟ€/4πœ‘πœ‹4\varphi\approx\pi/4italic_Ο† β‰ˆ italic_Ο€ / 4 for 1D sinusoidal modulations along any crystal direction. The real-space charge distribution that leads to the different EFGs for V1 to V3 cannot be extracted from the experimental results. Plausibly, the EFGs could display the imbalence of Fermi level states in the five V 3⁒d3𝑑3d3 italic_d orbitals related to the following discussion of the NMR shift. But they may also be affected by charges from bands below the Fermi energy and offsite contributions such as neighbored ions (e.g., the 3 Sn sites in Fig.Β 2) [37].

We further determined the NMR shift for two crystal orientations (aβˆ—superscriptπ‘Žβˆ—a^{\ast}italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT and cβˆ₯B0conditional𝑐subscript𝐡0c\parallel B_{0}italic_c βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT) and for a wide range of temperatures as shown in Fig.Β 4Β (C) and (D). For the analysis, we may separate the shift into two main components: (1) a very large and highly anisotropic part with a slight temperature dependence, and (2), the characteristic splitting as a consequence of the CDW phase transition. Component (1) is most likely dominated by a very large orbital shift (from 0.6Β %times0.6percent0.6\text{\,}\%start_ARG 0.6 end_ARG start_ARG times end_ARG start_ARG % end_ARG to well above 0.8Β %times0.8percent0.8\text{\,}\%start_ARG 0.8 end_ARG start_ARG times end_ARG start_ARG % end_ARG) stemming from the magnetic moment associated with the orbital motion of the electrons (van Vleck paramagnetism) that was repeatedly found in metallic V compounds [38, 39, 40, 41, 34, 42]. This shift term is typically independent of or weakly dependent on temperature, was reported to be insensitive to the CDW phase transition in 1T-VS2, and may thus explain why the total shift including its temperature dependence seems not to be directly related to the relaxation as expected from a Korringa relation (from K2⁒T1⁒T=c⁒o⁒n⁒s⁒t.superscript𝐾2subscript𝑇1π‘‡π‘π‘œπ‘›π‘ π‘‘K^{2}T_{1}T=const.italic_K start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT italic_T start_POSTSUBSCRIPT 1 end_POSTSUBSCRIPT italic_T = italic_c italic_o italic_n italic_s italic_t . we expect an isotropic shift of less than 0.1Β %times0.1percent0.1\text{\,}\%start_ARG 0.1 end_ARG start_ARG times end_ARG start_ARG % end_ARG with a distinct temperature dependence)Β [34, 42].

Refer to caption
Figure 6: NMR Shift and the modulation of the local DOS (A) The shift values from Fig.Β 4Β (A) plotted as Kcsubscript𝐾𝑐K_{c}italic_K start_POSTSUBSCRIPT italic_c end_POSTSUBSCRIPT vs. Kaβˆ—subscript𝐾superscriptπ‘Žβˆ—K_{a^{\ast}}italic_K start_POSTSUBSCRIPT italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT end_POSTSUBSCRIPT with the temperature as an intrinsic parameter. The red edged black square corresponds to 96Β Ktimes96K96\text{\,}\mathrm{K}start_ARG 96 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG, the red edged gray circle as well as the three 3d objects to 80Β Ktimes80K80\text{\,}\mathrm{K}start_ARG 80 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG. The dashed arrows indicate the direction of Ki⁒(T)subscript𝐾𝑖𝑇K_{i}(T)italic_K start_POSTSUBSCRIPT italic_i end_POSTSUBSCRIPT ( italic_T ) for decreasing temperatures. The black diagonal marks a line of constant isotropic NMR shift of 0.75Β %times0.75percent0.75\text{\,}\%start_ARG 0.75 end_ARG start_ARG times end_ARG start_ARG % end_ARG. (B) Orbital and site resolved DOS for high (black) and low (colored) temperatures from DFT. (C) The resulting sinusoidal modulation of the DOS for dx2βˆ’y2+dx⁒ysubscript𝑑superscriptπ‘₯2superscript𝑦2subscript𝑑π‘₯𝑦d_{x^{2}-y^{2}}+d_{xy}italic_d start_POSTSUBSCRIPT italic_x start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT - italic_y start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT end_POSTSUBSCRIPT + italic_d start_POSTSUBSCRIPT italic_x italic_y end_POSTSUBSCRIPT orbitals (l⁒e⁒f⁒t𝑙𝑒𝑓𝑑leftitalic_l italic_e italic_f italic_t) and the crystal aπ‘Žaitalic_a and b𝑏bitalic_b directions (equivalent) as well as for c𝑐citalic_c, beside V hourglass building blocks to illustrate the structural stacking of the V Kagome planes in the CDW phase (r⁒i⁒g⁒h⁒tπ‘Ÿπ‘–π‘”β„Žπ‘‘rightitalic_r italic_i italic_g italic_h italic_t). Colors denote crystal sites, i.e., V1 to V3, while the size of the balls represent the local DOS. The black solid and dashed boxes denote the unit cell for the high temperature and the CDW structure, respectively. (D) Similar to panel (C) for the dz2subscript𝑑superscript𝑧2d_{z^{2}}italic_d start_POSTSUBSCRIPT italic_z start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT end_POSTSUBSCRIPT orbitals and the corresponding modulation patterns of the local DOS. Obviously, the wavelength of the DOS modulation for dz2subscript𝑑superscript𝑧2d_{z^{2}}italic_d start_POSTSUBSCRIPT italic_z start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT end_POSTSUBSCRIPT orbitals is half the CDW unit cell in the crystal c𝑐citalic_c-direction, yielding an qz2=(13,13,23)subscriptπ‘žsuperscript𝑧2131323{q}_{z^{2}}=\left(\frac{1}{3},\frac{1}{3},\frac{2}{3}\right)italic_q start_POSTSUBSCRIPT italic_z start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT end_POSTSUBSCRIPT = ( divide start_ARG 1 end_ARG start_ARG 3 end_ARG , divide start_ARG 1 end_ARG start_ARG 3 end_ARG , divide start_ARG 2 end_ARG start_ARG 3 end_ARG ).

The second shift component (2) then contains all the changes due to the CDW phase. Obviously, the CDW phase emerges as an in good approximation temperature independent splitting of the single high temperature resonance line into a symmetric triplet of resonances for aβˆ—superscriptπ‘Žβˆ—a^{\ast}italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT and an asymmetric doublet for cβˆ₯B0conditional𝑐subscript𝐡0c\parallel B_{0}italic_c βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT. The switching between the two types of splittings appears unusual, but especially the two-fold splitting of three components in the cβˆ₯B0conditional𝑐subscript𝐡0c\parallel B_{0}italic_c βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT orientation is surprising, because it is not clear what causes such a symmetry breaking. To illustrate this puzzle, we show in Fig.Β 6Β (A) the shift data from Fig.Β 4 as a Kcsubscript𝐾𝑐K_{c}italic_K start_POSTSUBSCRIPT italic_c end_POSTSUBSCRIPT vs. Kaβˆ—subscript𝐾superscriptπ‘Žβˆ—K_{a^{\ast}}italic_K start_POSTSUBSCRIPT italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT end_POSTSUBSCRIPT-plot. The two shift patterns observed for c𝑐citalic_c and aβˆ—βˆ₯B0conditionalsuperscriptπ‘Žβˆ—subscript𝐡0a^{\ast}\parallel B_{0}italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT are sketched as projections on the two perpendicular axes (the 3d objects represent shift data at 80Β Ktimes80K80\text{\,}\mathrm{K}start_ARG 80 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG). They are fingerprints of commensurate 1D CDWs with q=1/3π‘ž13q=1/3italic_q = 1 / 3 that have a phase difference of Δ⁒φ=Ο€/2Ξ”πœ‘πœ‹2\Delta\varphi=\pi/2roman_Ξ” italic_Ο† = italic_Ο€ / 2 (cf. Fig.Β 1 C and D). The only difference between the two shift splittings is the orientation of the external field and it is rather unlikely that the field directly induces a phase change in the corresponding CDW. This raises the question for what causes the observed phase difference?

The shift anisotropy as a function of temperature brings some light into this problem. Beside the individual temperature dependencies drawn on the plane in Fig.Β 6Β (A) (color coding follows Fig.Β 4Β (C) and D), the red edged data points, representing K𝐾Kitalic_K just above (black - 96Β Ktimes96K96\text{\,}\mathrm{K}start_ARG 96 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG) and the averaged K𝐾Kitalic_K below (gray - 80Β Ktimes80K80\text{\,}\mathrm{K}start_ARG 80 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG) the CDW phase transition, are both located almost exactly on a line of constant isotropic shift of 0.75Β %times0.75percent0.75\text{\,}\%start_ARG 0.75 end_ARG start_ARG times end_ARG start_ARG % end_ARG. Under the reasonable assumption of axially symmetric shift tensors for both temperature regimes, the average isotropic shift thus remains unaffected by the phase transition, while the average axial component substantially changes (cf. Fig.Β 13 in the SI). Hence, the observed splittings in aβˆ—superscriptπ‘Žβˆ—a^{\ast}italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT and cβˆ₯B0conditional𝑐subscript𝐡0c\parallel B_{0}italic_c βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT are mainly caused by a splitting in the local electronic spin susceptibility (Pauli paramagnetism) with an anisotropic hyperfine interaction. Contact interaction and core polarization effects that yield isotropic NMR shifts cannot be responsible for the peculiar shift splittings. Spin dipolar interactions, on the other hand side, are highly anisotropic and may offer a way to resolve the conundrum of the phase shift between the two different field orientations [34, 43]. The shift measured for different field orientations could represent the shift contribution from orbitals with different geometry. In particular, the symmetric triplet in the plane may predominately arise from different DOS in the planar orbitals, i.e., dx2βˆ’y2subscript𝑑superscriptπ‘₯2superscript𝑦2d_{x^{2}-y^{2}}italic_d start_POSTSUBSCRIPT italic_x start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT - italic_y start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT end_POSTSUBSCRIPT and dx⁒ysubscript𝑑π‘₯𝑦d_{xy}italic_d start_POSTSUBSCRIPT italic_x italic_y end_POSTSUBSCRIPT, while the asymmetric doublet that appears with the field along the crystal c𝑐citalic_c-axis displays the DOS of the orbital with a distinct component along that direction, i.e.,Β dz2subscript𝑑superscript𝑧2d_{z^{2}}italic_d start_POSTSUBSCRIPT italic_z start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT end_POSTSUBSCRIPT.

To gain independent insight, we examined the DOS of individual orbitals for the 3 different V sites using DFT. The results are presented in Fig.Β 6Β (B) resolved for the sum of the dx2βˆ’y2+dx⁒ysubscript𝑑superscriptπ‘₯2superscript𝑦2subscript𝑑π‘₯𝑦d_{x^{2}-y^{2}}+d_{xy}italic_d start_POSTSUBSCRIPT italic_x start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT - italic_y start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT end_POSTSUBSCRIPT + italic_d start_POSTSUBSCRIPT italic_x italic_y end_POSTSUBSCRIPT orbitals (for symmetry reason both in-plane orbitals are equivalent), for dz2subscript𝑑superscript𝑧2d_{z^{2}}italic_d start_POSTSUBSCRIPT italic_z start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT end_POSTSUBSCRIPT, and for the dx⁒z+dy⁒zsubscript𝑑π‘₯𝑧subscript𝑑𝑦𝑧d_{xz}+d_{yz}italic_d start_POSTSUBSCRIPT italic_x italic_z end_POSTSUBSCRIPT + italic_d start_POSTSUBSCRIPT italic_y italic_z end_POSTSUBSCRIPT orbitals (again, both orbitals are equivalent). The site-selective DOS for the in-plane orbitals at the Fermi level splits symmetrically into 3 different DOS (purple, orange, and light blue), while for the out-of-plane orbital dz2subscript𝑑superscript𝑧2d_{z^{2}}italic_d start_POSTSUBSCRIPT italic_z start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT end_POSTSUBSCRIPT the splitting is two-fold, with V2 and V3 (orange and light blue) having almost exactly the same DOS. For dx⁒z+dy⁒zsubscript𝑑π‘₯𝑧subscript𝑑𝑦𝑧d_{xz}+d_{yz}italic_d start_POSTSUBSCRIPT italic_x italic_z end_POSTSUBSCRIPT + italic_d start_POSTSUBSCRIPT italic_y italic_z end_POSTSUBSCRIPT the three-fold splitting is again symmetric and visibly larger than for the other two components. Thus, DFT calculations almost perfectly reproduce the characteristic splittings observed with NMR, suggesting that the distinct orbital geometry is dominating the shift for special field orientations. Mapping the NMR/DFT data onto the low temperature crystal structure with V1, V2, and V3, we find the periodic, orbital specific modulations of the DOS as shown in panels (C) and (D) of Fig.Β 6. For dx2βˆ’y2+dx⁒ysubscript𝑑superscriptπ‘₯2superscript𝑦2subscript𝑑π‘₯𝑦d_{x^{2}-y^{2}}+d_{xy}italic_d start_POSTSUBSCRIPT italic_x start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT - italic_y start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT end_POSTSUBSCRIPT + italic_d start_POSTSUBSCRIPT italic_x italic_y end_POSTSUBSCRIPT orbitals, the corresponding wave vector is qx⁒y=(13,13,13)subscriptπ‘žπ‘₯𝑦131313{q}_{xy}=\left(\frac{1}{3},\frac{1}{3},\frac{1}{3}\right)italic_q start_POSTSUBSCRIPT italic_x italic_y end_POSTSUBSCRIPT = ( divide start_ARG 1 end_ARG start_ARG 3 end_ARG , divide start_ARG 1 end_ARG start_ARG 3 end_ARG , divide start_ARG 1 end_ARG start_ARG 3 end_ARG ) with a phase Ο†β‰ˆΟ€/2πœ‘πœ‹2\varphi\approx\pi/2italic_Ο† β‰ˆ italic_Ο€ / 2. The modulation for dx⁒z+dy⁒zsubscript𝑑π‘₯𝑧subscript𝑑𝑦𝑧d_{xz}+d_{yz}italic_d start_POSTSUBSCRIPT italic_x italic_z end_POSTSUBSCRIPT + italic_d start_POSTSUBSCRIPT italic_y italic_z end_POSTSUBSCRIPT orbitals (not shown) has the same wave vector but Ο†β‰ˆΟ€/6πœ‘πœ‹6\varphi\approx\pi/6italic_Ο† β‰ˆ italic_Ο€ / 6. Due to the twofold splitting in the dz2subscript𝑑superscript𝑧2d_{z^{2}}italic_d start_POSTSUBSCRIPT italic_z start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT end_POSTSUBSCRIPT orbitals, the corresponding modulation is characterized by qz2=(13,13,23)subscriptπ‘žsuperscript𝑧2131323{q}_{z^{2}}=\left(\frac{1}{3},\frac{1}{3},\frac{2}{3}\right)italic_q start_POSTSUBSCRIPT italic_z start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT end_POSTSUBSCRIPT = ( divide start_ARG 1 end_ARG start_ARG 3 end_ARG , divide start_ARG 1 end_ARG start_ARG 3 end_ARG , divide start_ARG 2 end_ARG start_ARG 3 end_ARG ) and Ο†β‰ˆ0πœ‘0\varphi\approx 0italic_Ο† β‰ˆ 0. Thus, NMR and DFT imply orbital specific modulations of the DOS that differ in amplitude, phase, and, in case of the V dz2subscript𝑑superscript𝑧2d_{z^{2}}italic_d start_POSTSUBSCRIPT italic_z start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT end_POSTSUBSCRIPT modulation, even in periodicity of the out-of-plane component. In this scenario, the switching between the in-plane orbitals and the out-of-plane orbitals requires a highly selective hyperfine interaction. This should be subject of a theoretical investigation in future studies. Finally, the chirality of the crystal structure is transferred to the modulations of the DOS where corner-sharing triangular columns (light and dark gray) have opposite handedness.

The CDW phase transition and fluctuations of the local magnetic field For a metallic system like ScV6Sn6, the spin-relaxation is typically governed by magnetic relaxation, i.e., by fluctuations of the local magnetic field arising from conduction electrons (cf. the corresponding section and Fig.Β 16 in the SI). The temperature dependence of the relaxation rate 1/T11subscript𝑇11/T_{1}1 / italic_T start_POSTSUBSCRIPT 1 end_POSTSUBSCRIPT should then be proportional to the square of the DOS (Korringa relation). We evaluated the following integral,

1T1∝Ahf2⁒∫f⁒(Eβˆ’ΞΌc)⁒[1βˆ’f⁒(Eβˆ’ΞΌc)]⁒D⁒(E)2⁒dE,proportional-to1subscript𝑇1subscriptsuperscript𝐴2hf𝑓𝐸subscriptπœ‡π‘delimited-[]1𝑓𝐸subscriptπœ‡π‘π·superscript𝐸2differential-d𝐸\frac{1}{T_{1}}\propto A^{2}_{\mathrm{hf}}\int f(E-\mu_{c})[1-f(E-\mu_{c})]D(E% )^{2}\mathrm{d}E\ ,divide start_ARG 1 end_ARG start_ARG italic_T start_POSTSUBSCRIPT 1 end_POSTSUBSCRIPT end_ARG ∝ italic_A start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT start_POSTSUBSCRIPT roman_hf end_POSTSUBSCRIPT ∫ italic_f ( italic_E - italic_ΞΌ start_POSTSUBSCRIPT italic_c end_POSTSUBSCRIPT ) [ 1 - italic_f ( italic_E - italic_ΞΌ start_POSTSUBSCRIPT italic_c end_POSTSUBSCRIPT ) ] italic_D ( italic_E ) start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT roman_d italic_E , (5)

where Ahfsubscript𝐴hfA_{\mathrm{hf}}italic_A start_POSTSUBSCRIPT roman_hf end_POSTSUBSCRIPT represents the hyperfine interaction that we assume to be temperature independent, f⁒(E)𝑓𝐸f(E)italic_f ( italic_E ) denotes the Fermi function, ΞΌcsubscriptπœ‡π‘\mu_{c}italic_ΞΌ start_POSTSUBSCRIPT italic_c end_POSTSUBSCRIPT the temperature dependent chemical potential, and D⁒(E)𝐷𝐸D(E)italic_D ( italic_E ) the energy dependence of the DOS for the high and the low temperature phase from the inset of Fig.Β 5Β (A). The results are shown by the dashed and the solid black line in Fig.Β 5Β (A) after appropriate rescaling. We find a very good agreement between experimental results and DFT. That is, the nuclear spins see the electronic states at the Fermi level and relax via their excitations, while the temperature limits the available states through the Fermi function (∼kB⁒Tsimilar-toabsentsubscriptπ‘˜B𝑇\sim k_{\mathrm{B}}T∼ italic_k start_POSTSUBSCRIPT roman_B end_POSTSUBSCRIPT italic_T). As mentioned in the results section, the relaxation rate values in the CDW phase denote the average of the 3 individual resonance lines, and similarly the low temperature DOS in panel (A) are not resolved for the 3 V sites. It may thus be possible that the relaxation also shows differences among the 3 V sites similar to the shift values. This, however, could not reliably be resolved with experiment.

A different way to look at the relaxation data is presented in Fig.Β 5 (B) where the 1/T1⁒T⁒(T)1subscript𝑇1𝑇𝑇1/T_{1}T(T)1 / italic_T start_POSTSUBSCRIPT 1 end_POSTSUBSCRIPT italic_T ( italic_T ) is separated into 3 parts, Fermi liquid behavior below and above the CDW phase transition separated by a change in DOS by a factor of 22\sqrt{2}square-root start_ARG 2 end_ARG, and a high temperature dependence above 150Β Ktimes150K150\text{\,}\mathrm{K}start_ARG 150 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG that can very well be approximated by an activation-type of behavior. A single exponential fit yields a gap of the size of about 160Β meVtimes160meV160\text{\,}\mathrm{m}\mathrm{e}\mathrm{V}start_ARG 160 end_ARG start_ARG times end_ARG start_ARG roman_meV end_ARG (cf. Arrhenius plot in panel C) which might be relatable to band structure features, such as van Hove singularities as suggested by others [44]. In the current case of ScV6Sn6, however, the band structure is too complex to unambiguously relate the spin-lattice relaxation to individual bands and their dispersion.

Conclusions

We investigated the CDW Kagome metal ScV6Sn6 using single crystal 51V NMR and DFT. The CDW phase transition occurs between 96Β times96absent96\text{\,}start_ARG 96 end_ARG start_ARG times end_ARG start_ARG end_ARG and about 80Β Ktimes80K80\text{\,}\mathrm{K}start_ARG 80 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG and takes place as a gradual replacement of the high temperature phase by the CDW phase as expected from a first order transition. The phase transition is accompanied by a change in the electronic band structure and the corresponding changes in the total DOS by a factor of 22\sqrt{2}square-root start_ARG 2 end_ARG is very well reproduced with DFT to match the experimentally observed evolution of the local magnetic field fluctuations for decreasing temperatures. The CDW phase features an individual conversion of the three formerly equivalent V environments per V triangle in agreement with DFT and the reported reconstruction of the unit cell with 3Γ—3Γ—3333\sqrt{3}\times\sqrt{3}\times 3square-root start_ARG 3 end_ARG Γ— square-root start_ARG 3 end_ARG Γ— 3 periodicity. In the CDW phase, our findings further comprise an unusual orientation dependent change in the NMR shift splitting from a symmetric triplet of resonance lines for aβˆ—βˆ₯B0conditionalsuperscriptπ‘Žβˆ—subscript𝐡0a^{\ast}\parallel B_{0}italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT to a asymmetric doublet for cβˆ₯B0conditional𝑐subscript𝐡0c\parallel B_{0}italic_c βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT, while the latter reflects a symmetry that cannot be found in the crystal structure. When regarded as one-dimensional sinusoidal modulations of the local magnetic field, this observation implies a magnetic field induced phase shift of Δ⁒φ=Ο€/2Ξ”πœ‘πœ‹2\Delta\varphi=\pi/2roman_Ξ” italic_Ο† = italic_Ο€ / 2. To resolve this discrepancy, we argue on the basis of orbital selective modulations of the local DOS with in-plane wave vector q=(13,13)π‘ž1313q=\left(\frac{1}{3},\frac{1}{3}\right)italic_q = ( divide start_ARG 1 end_ARG start_ARG 3 end_ARG , divide start_ARG 1 end_ARG start_ARG 3 end_ARG ) but different out-of-plane wave vectors and phases, driven by a field orientation selective hyperfine coupling. The latter calls for a quantitative theoretical treatment of the hyperfine interaction and possible implications for the compound’s transport properties. Our work demonstrates that the combination of single crystal NMR and DFT calculations leads to crucial local information about static and dynamic electronic properties in the charge density wave system ScV6Sn6.

Methods

Crystal synthesis High-quality single crystals of ScV6Sn6 were grown by the flux method [5]. High-purity Sc, V, and Sn elements were loaded in an alumina crucible in a molar ratio of 1Β :Β 10Β :Β 60 and then sealed in a quartz tube under vacuum. The tube was then slowly heated to 1373 K, maintained for 10 h, and cooled down to 973 K over 400 h. Hexagonal shape crystals with silvery surfaces and a typical size of 2Γ—2Γ—1⁒ mm3221timesabsentsuperscriptmm32\times 2\times 1$\text{\,}\mathrm{m}\mathrm{m}^{3}$2 Γ— 2 Γ— 1 start_ARG end_ARG start_ARG times end_ARG start_ARG roman_mm start_POSTSUPERSCRIPT 3 end_POSTSUPERSCRIPT end_ARG were obtained after centrifugation. The crystal structure was refined from powder x-ray diffraction and the chemical components were examined by using energy-dispersive X-ray spectroscopy The crystal orientations were determined by using the Laue backscattering diffractometer.

NMR experiments Measurements were carried out on a Janis sweepable 9Β Ttimes9T9\text{\,}\mathrm{T}start_ARG 9 end_ARG start_ARG times end_ARG start_ARG roman_T end_ARG magnet and a Tecmag Apollo NMR console. Most experiments were carried out on the hexagonal, plate-like Sample S2 with dimensions 1.7Β Γ—1.1Β Γ—0.2Β mm3times1.7absenttimes1.1absenttimes0.2superscriptmm3$1.7\text{\,}$\times$1.1\text{\,}$\times$0.2\text{\,}\mathrm{m}\mathrm{m}^{3}$start_ARG 1.7 end_ARG start_ARG times end_ARG start_ARG end_ARG Γ— start_ARG 1.1 end_ARG start_ARG times end_ARG start_ARG end_ARG Γ— start_ARG 0.2 end_ARG start_ARG times end_ARG start_ARG roman_mm start_POSTSUPERSCRIPT 3 end_POSTSUPERSCRIPT end_ARG (cf. Yi et al. 2024 [15]). A few measurements were done on Sample S1 with 1.5Β Γ—0.45Β Γ—0.15Β mm3times1.5absenttimes0.45absenttimes0.15superscriptmm3$1.5\text{\,}$\times$0.45\text{\,}$\times$0.15\text{\,}\mathrm{m}\mathrm{m}^{3}$start_ARG 1.5 end_ARG start_ARG times end_ARG start_ARG end_ARG Γ— start_ARG 0.45 end_ARG start_ARG times end_ARG start_ARG end_ARG Γ— start_ARG 0.15 end_ARG start_ARG times end_ARG start_ARG roman_mm start_POSTSUPERSCRIPT 3 end_POSTSUPERSCRIPT end_ARG. In both cases, the rf-coil was wound directly around the sample and placed on the single axis goniometer (accuracy ∼similar-to\sim∼1Β Β°times1degree1\text{\,}\mathrm{\SIUnitSymbolDegree}start_ARG 1 end_ARG start_ARG times end_ARG start_ARG Β° end_ARG) of a home-built probe. Most experiments were carried out at 8.73Β Ttimes8.73T8.73\text{\,}\mathrm{T}start_ARG 8.73 end_ARG start_ARG times end_ARG start_ARG roman_T end_ARG typically using broad-band free induction decay (FID) measurements with pulse lengths of 0.5 μ⁒stimes0.5πœ‡s0.5\text{\,}\mu\mathrm{s}start_ARG 0.5 end_ARG start_ARG times end_ARG start_ARG italic_ΞΌ roman_s end_ARG in combination with low Q𝑄Qitalic_Q-factors (in the order of 10), as well as selective FID or spin-echo (Ο€/2βˆ’Ο„βˆ’Ο€πœ‹2πœπœ‹\pi/2-\tau-\piitalic_Ο€ / 2 - italic_Ο„ - italic_Ο€) experiments with Ο€/2πœ‹2\pi/2italic_Ο€ / 2-pulse lengths of 5 or 10 μ⁒stimes10πœ‡s10\text{\,}\mu\mathrm{s}start_ARG 10 end_ARG start_ARG times end_ARG start_ARG italic_ΞΌ roman_s end_ARG for individual resonance lines (Q𝑄Qitalic_Q between 16 and 32, cf. SI). Selective saturation recovery pulse sequence (Ο€/2βˆ’Ξ”βˆ’πœ‹2limit-fromΞ”\pi/2-\Delta-italic_Ο€ / 2 - roman_Ξ” -FID/spin echo) was employed to measure the spin-lattice relaxation time T1subscript𝑇1T_{1}italic_T start_POSTSUBSCRIPT 1 end_POSTSUBSCRIPT of individual transitions. The shifts were obtained by referencing the 51V resonance frequencies versus VOCl3 using the second reference method [45] and the omnipresent 63Cu resonance line of the rf-coil.

Numerical calculations The simulated results were obtained by using ab initio calculations in the framework of density-functional theory (DFT), as implemented in the program VASPΒ [35]. In this code, augmented plane waves are used as a basis set together with pseudopotentials. To describe the exchange-correlation potential, the generalized-gradient approximation (GGA)Β [46] was used.

The EFGs and self-consistent calculations were carried out on a 18Γ—18Γ—91818918\times 18\times 918 Γ— 18 Γ— 9 (6Γ—6Γ—66666\times 6\times 66 Γ— 6 Γ— 6) k mesh for the high (low) temperature phase, respectively. Convergence for total energy and EFGs was carefully checked. For the DOS calculations, a k mesh of 33Γ—33Γ—3333333333\times 33\times 3333 Γ— 33 Γ— 33 (19Γ—19Γ—1919191919\times 19\times 1919 Γ— 19 Γ— 19) was used for the high (low) temperature phase, respectively.

Data availability

The data that support the findings of this study are available from the corresponding authors upon reasonable request.

Code availability

The codes that support the findings of this study are available from the corresponding authors upon reasonable request.

Acknowledgment

The authors thank O. Stockert, S. Wirth, J. Sichelschmidt, X. Feng, W. Schnelle, and J. Haase (Leipzig) for helpful discussions. We acknowledge the financial support by the Deutsche Forschungsgemeinschaft (DFG) under SFB1143 (Project No. 247310070), the WΓΌrzburg-Dresden Cluster of Excellence on Complexity and Topology in Quantum Matterβ€”ct.qmat (EXC 2147, Project No. 390858490). M.G.V. acknowledges support to the Spanish Ministerio de Ciencia e Innovacion (grant PID2022-142008NB-I00), partial support from European Research Council (ERC) grant agreement no. 101020833, the European Union NextGenerationEU/PRTR-C17.I1, by the IKUR Strategy under the collaboration agreement between Ikerbasque Foundation and DIPC on behalf of the Department of Education of the Basque Government and the Ministry for Digital Transformation and of Civil Service of the Spanish Government through the QUANTUM ENIA project call - Quantum Spain project, and by the European Union through the Recovery, Transformation and Resilience Plan - NextGenerationEU within the framework of the Digital Spain 2026 Agenda. M.G.V. and C.F. acknowledge funding from the Deutsche Forschungsgemeinschaft (DFG, German Research Foundation) for the project FOR 5249 (QUAST).

Author contributions

R.G performed NMR experiments, analyzed data, and wrote the manuscript. M.B. assisted in the NMR experiments and worked with R.G. on the interpretation of the NMR data. J.N. performed theoretical calculations. J.N. and M.G. assisted in data analysis. C.Y. and S.C. grew and characterized single crystals. C.F supervised the project. All authors commented on the manuscript.

Competing interest

The authors declare no competing interests.

Additional information

The Supplementary information is attached at the end of this manuscript.

References

  • WilsonΒ andΒ Ortiz [2023] S.Β D.Β WilsonΒ andΒ B.Β R.Β Ortiz,Β AV3Sb5 Kagome Superconductors: Progress and Future Directions,Β arXiv preprint arXiv:2311.05946Β  (2023).
  • GuoΒ etΒ al. [2022] C.Β Guo, C.Β Putzke, S.Β Konyzheva, X.Β Huang, M.Β Gutierrez-Amigo, I.Β Errea, D.Β Chen, M.Β G.Β Vergniory, C.Β Felser, M.Β H.Β Fischer, etΒ al.,Β Switchable chiral transport in charge-ordered kagome metal CsV3Sb5,Β NatureΒ 611,Β 461 (2022).
  • MielkeΒ IIIΒ etΒ al. [2022] C.Β MielkeΒ III, D.Β Das, J.-X.Β Yin, H.Β Liu, R.Β Gupta, Y.-X.Β Jiang, M.Β Medarde, X.Β Wu, H.Β C.Β Lei, J.Β Chang, etΒ al.,Β Time-reversal symmetry-breaking charge order in a kagome superconductor,Β NatureΒ 602,Β 245 (2022).
  • ZhangΒ etΒ al. [2022] X.Β Zhang, J.Β Hou, W.Β Xia, Z.Β Xu, P.Β Yang, A.Β Wang, Z.Β Liu, J.Β Shen, H.Β Zhang, X.Β Dong, Y.Β Uwatoko, J.Β Sun, B.Β Wang, Y.Β Guo,Β andΒ J.Β Cheng,Β Destabilization of the Charge Density Wave and the Absence of Superconductivity in ScV6Sn6 under High Pressures up to 11 GPa,Β MaterialsΒ 15,Β 10.3390/ma15207372 (2022),Β https://www.mdpi.com/1996-1944/15/20/7372 .
  • ArachchigeΒ etΒ al. [2022] H.Β W.Β S.Β Arachchige, W.Β R.Β Meier, M.Β Marshall, T.Β Matsuoka, R.Β Xue, M.Β A.Β McGuire, R.Β P.Β Hermann, H.Β Cao,Β andΒ D.Β Mandrus,Β Charge Density Wave in Kagome Lattice Intermetallic ScV6⁒Sn6subscriptScV6subscriptSn6{\mathrm{ScV}}_{6}{\mathrm{Sn}}_{6}roman_ScV start_POSTSUBSCRIPT 6 end_POSTSUBSCRIPT roman_Sn start_POSTSUBSCRIPT 6 end_POSTSUBSCRIPT,Β Phys. Rev. Lett.Β 129,Β 216402 (2022),Β https://link.aps.org/doi/10.1103/PhysRevLett.129.216402 .
  • GuΒ etΒ al. [2023] Y.Β Gu, E.Β T.Β Ritz, W.Β R.Β Meier, A.Β Blockmon, K.Β Smith, R.Β P.Β Madhogaria, S.Β Mozaffari, D.Β Mandrus, T.Β Birol,Β andΒ J.Β L.Β Musfeldt,Β Phonon mixing in the charge density wave state of ScV6⁒Sn6subscriptScV6subscriptSn6{\mathrm{ScV}}_{6}{\mathrm{Sn}}_{6}roman_ScV start_POSTSUBSCRIPT 6 end_POSTSUBSCRIPT roman_Sn start_POSTSUBSCRIPT 6 end_POSTSUBSCRIPT,Β npj Quantum Mater.Β 8,Β 58 (2023).
  • TunizΒ etΒ al. [2023] M.Β Tuniz, A.Β Consiglio, D.Β Puntel, C.Β Bigi, S.Β Enzner, G.Β Pokharel, P.Β Orgiani, W.Β Bronsch, F.Β Parmigiani, V.Β Polewczyk, etΒ al.,Β Dynamics and resilience of the unconventional charge density wave in ScV6Sn6 bilayer kagome metal,Β Commun. Mater.Β 4,Β 103 (2023).
  • HuΒ etΒ al. [2023] H.Β Hu, Y.Β Jiang, D.Β CΔƒlugΔƒru, X.Β Feng, D.Β Subires, M.Β G.Β Vergniory, C.Β Felser, S.Β Blanco-Canosa,Β andΒ B.Β A.Β Bernevig,Β Kagome Materials I: SG 191, ScV6Sn6. Flat Phonon Soft Modes and Unconventional CDW Formation: Microscopic and Effective Theory,Β arXiv preprint arXiv:2305.15469Β  (2023).
  • TanΒ andΒ Yan [2023] H.Β TanΒ andΒ B.Β Yan,Β Abundant lattice instability in kagome metal scv6⁒sn6subscriptscv6subscriptsn6{\mathrm{scv}}_{6}{\mathrm{sn}}_{6}roman_scv start_POSTSUBSCRIPT 6 end_POSTSUBSCRIPT roman_sn start_POSTSUBSCRIPT 6 end_POSTSUBSCRIPT,Β Phys. Rev. Lett.Β 130,Β 266402 (2023).
  • PokharelΒ etΒ al. [2023] G.Β Pokharel, B.Β R.Β Ortiz, L.Β Kautzsch, S.Β J.Β GomezΒ Alvarado, K.Β Mallayya, G.Β Wu, E.-A.Β Kim, J.Β P.Β C.Β Ruff, S.Β Sarker,Β andΒ S.Β D.Β Wilson,Β Frustrated charge order and cooperative distortions in ScV6⁒Sn6subscriptScV6subscriptSn6{\mathrm{ScV}}_{6}{\mathrm{Sn}}_{6}roman_ScV start_POSTSUBSCRIPT 6 end_POSTSUBSCRIPT roman_Sn start_POSTSUBSCRIPT 6 end_POSTSUBSCRIPT,Β Phys. Rev. Mater.Β 7,Β 104201 (2023),Β https://link.aps.org/doi/10.1103/PhysRevMaterials.7.104201 .
  • KorshunovΒ etΒ al. [2023] A.Β Korshunov, H.Β Hu, D.Β Subires, Y.Β Jiang, D.Β CΔƒlugΔƒru, X.Β Feng, A.Β Rajapitamahuni, C.Β Yi, S.Β Roychowdhury, M.Β G.Β Vergniory, J.Β Strempfer, C.Β Shekhar, E.Β Vescovo, D.Β Chernyshov, A.Β H.Β Said, A.Β Bosak, C.Β Felser, B.Β A.Β Bernevig,Β andΒ S.Β Blanco-Canosa,Β Softening of a flat phonon mode in the kagome ScV6Sn6,Β Nat. Commun.Β 14,Β 10.1038/s41467-023-42186-6 (2023),Β http://dx.doi.org/10.1038/s41467-023-42186-6 .
  • KimΒ etΒ al. [2023] D.Β W.Β Kim, S.Β Liu, C.Β Wang, H.Β W.Β Nam, G.Β Pokharel, S.Β D.Β Wilson, J.-H.Β Cho,Β andΒ S.Β J.Β Moon,Β Infrared probe of the charge density wave gap in ScV6⁒Sn6subscriptScV6subscriptSn6\mathrm{Sc}{\mathrm{V}}_{6}{\mathrm{Sn}}_{6}roman_ScV start_POSTSUBSCRIPT 6 end_POSTSUBSCRIPT roman_Sn start_POSTSUBSCRIPT 6 end_POSTSUBSCRIPT,Β Phys. Rev. BΒ 108,Β 205118 (2023),Β https://link.aps.org/doi/10.1103/PhysRevB.108.205118 .
  • CaoΒ etΒ al. [2023] S.Β Cao, C.Β Xu, H.Β Fukui, T.Β Manjo, Y.Β Dong, M.Β Shi, Y.Β Liu, C.Β Cao,Β andΒ Y.Β Song,Β Competing charge-density wave instabilities in the kagome metal ScV6Sn6,Β Nat. Commun.Β 14,Β 10.1038/s41467-023-43454-1 (2023),Β http://dx.doi.org/10.1038/s41467-023-43454-1 .
  • ShresthaΒ etΒ al. [2023] K.Β Shrestha, B.Β Regmi, G.Β Pokharel, S.-G.Β Kim, S.Β D.Β Wilson, D.Β E.Β Graf, B.Β A.Β Magar, C.Β Phillips,Β andΒ T.Β Nguyen,Β Electronic properties of kagome metal ScV6⁒Sn6subscriptScV6subscriptSn6{\mathrm{ScV}}_{6}{\mathrm{Sn}}_{6}roman_ScV start_POSTSUBSCRIPT 6 end_POSTSUBSCRIPT roman_Sn start_POSTSUBSCRIPT 6 end_POSTSUBSCRIPT using high-field torque magnetometry,Β Phys. Rev. BΒ 108,Β 245119 (2023),Β https://link.aps.org/doi/10.1103/PhysRevB.108.245119 .
  • YiΒ etΒ al. [2024] C.Β Yi, X.Β Feng, N.Β Mao, P.Β Yanda, S.Β Roychowdhury, Y.Β Zhang, C.Β Felser,Β andΒ C.Β Shekhar,Β Quantum oscillations revealing topological band in kagome metal ScV6⁒Sn6subscriptScV6subscriptSn6{\mathrm{ScV}}_{6}{\mathrm{Sn}}_{6}roman_ScV start_POSTSUBSCRIPT 6 end_POSTSUBSCRIPT roman_Sn start_POSTSUBSCRIPT 6 end_POSTSUBSCRIPT,Β Phys. Rev. BΒ 109,Β 035124 (2024),Β https://link.aps.org/doi/10.1103/PhysRevB.109.035124 .
  • ChengΒ etΒ al. [2024a] Z.-J.Β Cheng, S.Β Shao, B.Β Kim, T.Β A.Β Cochran, X.Β P.Β Yang, C.Β Yi, Y.-X.Β Jiang, J.Β Zhang, M.Β S.Β Hossain, S.Β Roychowdhury, T.Β Yilmaz, E.Β Vescovo, A.Β Fedorov, C.Β Shekhar, C.Β Felser, G.Β Chang,Β andΒ M.Β Z.Β Hasan,Β Untangling charge-order dependent bulk states from surface effects in a topological kagome metal ScV6⁒Sn6subscriptScV6subscriptSn6{\mathrm{ScV}}_{6}{\mathrm{Sn}}_{6}roman_ScV start_POSTSUBSCRIPT 6 end_POSTSUBSCRIPT roman_Sn start_POSTSUBSCRIPT 6 end_POSTSUBSCRIPT,Β Phys. Rev. BΒ 109,Β 075150 (2024a),Β https://link.aps.org/doi/10.1103/PhysRevB.109.075150 .
  • LeeΒ etΒ al. [2024] S.Β Lee, C.Β Won, J.Β Kim, J.Β Yoo, S.Β Park, J.Β Denlinger, C.Β Jozwiak, A.Β Bostwick, E.Β Rotenberg, R.Β Comin, etΒ al.,Β Nature of charge density wave in kagome metal ScV6Sn6,Β npj Quantum Mater.Β 9,Β 15 (2024).
  • Subedi [2024] A.Β Subedi,Β Order-by-disorder charge density wave condensation at q=(13,13,13)π‘ž131313\mathit{q}=(\frac{1}{3},\frac{1}{3},\frac{1}{3})italic_q = ( divide start_ARG 1 end_ARG start_ARG 3 end_ARG , divide start_ARG 1 end_ARG start_ARG 3 end_ARG , divide start_ARG 1 end_ARG start_ARG 3 end_ARG ) in kagome metal ScV6⁒Sn6subscriptScV6subscriptSn6{\mathrm{ScV}}_{6}{\mathrm{Sn}}_{6}roman_ScV start_POSTSUBSCRIPT 6 end_POSTSUBSCRIPT roman_Sn start_POSTSUBSCRIPT 6 end_POSTSUBSCRIPT,Β Phys. Rev. Mater.Β 8,Β 014006 (2024),Β https://link.aps.org/doi/10.1103/PhysRevMaterials.8.014006 .
  • HuΒ etΒ al. [2024] Y.Β Hu, J.Β Ma, Y.Β Li, Y.Β Jiang, D.Β J.Β Gawryluk, T.Β Hu, J.Β Teyssier, V.Β Multian, Z.Β Yin, S.Β Xu, etΒ al.,Β Phonon promoted charge density wave in topological kagome metal ScV6Sn6,Β Nat. Commun.Β 15,Β 1658 (2024).
  • YangΒ etΒ al. [2024] Y.-C.Β Yang, S.Β Cho, T.-R.Β Li, X.-Q.Β Liu, Z.-T.Β Liu, Z.-C.Β Jiang, J.-Y.Β Ding, W.Β Xia, Z.-C.Β Tao, J.-Y.Β Liu, etΒ al.,Β Unveiling the charge density wave mechanism in vanadium-based Bi-layered kagome metals,Β arXiv preprint arXiv:2402.03765Β  (2024).
  • WangΒ etΒ al. [2024] K.Β Wang, S.Β Chen, S.-W.Β Kim,Β andΒ B.Β Monserrat,Β Origin of competing charge density waves in kagome metal ScV6Sn6,Β arXiv preprint arXiv:2403.17058Β  (2024).
  • ChengΒ etΒ al. [2024b] S.Β Cheng, Z.Β Ren, H.Β Li, J.Β S.Β Oh, H.Β Tan, G.Β Pokharel, J.Β M.Β DeStefano, E.Β Rosenberg, Y.Β Guo, Y.Β Zhang, etΒ al.,Β Nanoscale visualization and spectral fingerprints of the charge order in ScV6Sn6 distinct from other kagome metals,Β npj Quantum Mater.Β 9,Β 14 (2024b).
  • ZhengΒ etΒ al. [2024] G.Β Zheng, Y.Β Zhu, S.Β Mozaffari, N.Β Mao, K.-W.Β Chen, K.Β Jenkins, D.Β Zhang, A.Β Chan, H.Β W.Β S.Β Arachchige, R.Β P.Β Madhogaria, M.Β Cothrine, W.Β R.Β Meier, Y.Β Zhang, D.Β Mandrus,Β andΒ L.Β Li,Β Quantum oscillations evidence for topological bands in kagome metal ScV6Sn6,Β J. Phys.: Condens. MatterΒ 36,Β 215501 (2024),Β https://dx.doi.org/10.1088/1361-648X/ad2803 .
  • GuguchiaΒ etΒ al. [2023] Z.Β Guguchia, D.Β Gawryluk, S.Β Shin, Z.Β Hao, C.Β MielkeΒ III, D.Β Das, I.Β Plokhikh, L.Β Liborio, J.Β K.Β Shenton, Y.Β Hu, etΒ al.,Β Hidden magnetism uncovered in a charge ordered bilayer kagome material ScV6Sn6,Β Nat. Commun.Β 14,Β 7796 (2023).
  • Butz [1992] T.Β Butz,Β ed.,Β Nuclear spectroscopy and charge density wave systems,Β Physics and chemistry of materials with low-dimensional structures, Vol.Β 15Β (Kluwer Academic Publishers,Β 1992).
  • VendittiΒ andΒ Caprara [2023] G.Β VendittiΒ andΒ S.Β Caprara,Β Charge-density waves vs. superconductivity: Some results and future perspectives,Β Condens. MatterΒ 8,Β 54 (2023),Β http://dx.doi.org/10.3390/condmat8030054 .
  • VinogradΒ etΒ al. [2021] I.Β Vinograd, R.Β Zhou, M.Β Hirata, T.Β Wu, H.Β Mayaffre, S.Β KrΓ€mer, R.Β Liang, W.Β N.Β Hardy, D.Β A.Β Bonn,Β andΒ M.-H.Β Julien,Β Locally commensurate charge-density wave with three-unit-cell periodicity in YBa2Cu3Oy,Β Nat. Commun.Β 12 (2021),Β http://dx.doi.org/10.1038/s41467-021-23140-w .
  • ZhengΒ etΒ al. [2022] L.Β Zheng, Z.Β Wu, Y.Β Yang, L.Β Nie, M.Β Shan, K.Β Sun, D.Β Song, F.Β Yu, J.Β Li, D.Β Zhao, etΒ al.,Β Emergent charge order in pressurized kagome superconductor CsV3Sb5,Β NatureΒ 611,Β 682 (2022),Β https://doi.org/10.1038/s41586-022-05351-3 .
  • LuoΒ etΒ al. [2022] J.Β Luo, Z.Β Zhao, Y.Β Zhou, J.Β Yang, A.Β Fang, H.Β Yang, H.Β Gao, R.Β Zhou,Β andΒ G.-q.Β Zheng,Β Possible star-of-David pattern charge density wave with additional modulation in the kagome superconductor CsV3Sb5,Β npj Quantum Mater.Β 7,Β 30 (2022),Β https://doi.org/10.1038/s41535-022-00437-7 .
  • SongΒ etΒ al. [2022] D.Β Song, L.Β Zheng, F.Β Yu, J.Β Li, L.Β Nie, M.Β Shan, D.Β Zhao, S.Β Li, B.Β Kang, Z.Β Wu, etΒ al.,Β Orbital ordering and fluctuations in a kagome superconductor CsV3Sb5,Β Sci. China: Phys., Mech. Astron.Β 65,Β 247462 (2022),Β https://doi.org/10.1007/s11433-021-1826-1 .
  • MuΒ etΒ al. [2021] C.Β Mu, Q.Β Yin, Z.Β Tu, C.Β Gong, H.Β Lei, Z.Β Li,Β andΒ J.Β Luo,Β S-Wave Superconductivity in Kagome Metal CsV3Sb5 Revealed by 121/123Sb NQR and 51V NMR Measurements,Β Chin. Phys. Lett.Β 38,Β 077402 (2021),Β https://dx.doi.org/10.1088/0256-307X/38/7/077402 .
  • FollstaedtΒ andΒ Slichter [1976] D.Β FollstaedtΒ andΒ C.Β P.Β Slichter,Β NMR search for charge density waves,Β Phys. Rev. BΒ 13,Β 1017–1027 (1976),Β http://dx.doi.org/10.1103/PhysRevB.13.1017 .
  • GrΓΌner [1988] G.Β GrΓΌner,Β The dynamics of charge-density waves,Β Rev. Mod. Phys.Β 60,Β 1129 (1988).
  • BennettΒ etΒ al. [1970] L.Β Bennett, R.Β Watson,Β andΒ G.Β Carter,Β Relevance of knight shift measurements to the electronic density of states,Β J. Res. Natl. Bur. Stand. A Phys. Chem.Β 74A,Β 569 (1970),Β http://dx.doi.org/10.6028/jres.074A.048 .
  • KresseΒ andΒ FurthmΓΌller [1996] G.Β KresseΒ andΒ J.Β FurthmΓΌller,Β Efficient iterative schemes for ab initio total-energy calculations using a plane-wave basis set,Β Phys. Rev. BΒ 54,Β 11169 (1996),Β arXiv:0927-0256(96)00008 .
  • PetrilliΒ etΒ al. [1998] H.Β M.Β Petrilli, P.Β E.Β BlΓΆchl, P.Β Blaha,Β andΒ K.Β Schwarz,Β Electric-field-gradient calculations using the projector augmented wave method,Β Phys. Rev. BΒ 57,Β 14690 (1998).
  • GuehneΒ andΒ Chlan [2024] R.Β GuehneΒ andΒ V.Β c.Β v.Β Chlan,Β Exploring the nontrivial band edge in the bulk of the topological insulators bi2⁒se3subscriptbi2subscriptse3{\mathrm{bi}}_{2}{\mathrm{se}}_{3}roman_bi start_POSTSUBSCRIPT 2 end_POSTSUBSCRIPT roman_se start_POSTSUBSCRIPT 3 end_POSTSUBSCRIPT and bi2⁒te3subscriptbi2subscriptte3{\mathrm{bi}}_{2}{\mathrm{te}}_{3}roman_bi start_POSTSUBSCRIPT 2 end_POSTSUBSCRIPT roman_te start_POSTSUBSCRIPT 3 end_POSTSUBSCRIPT,Β Phys. Rev. Res.Β 6,Β 013214 (2024),Β https://link.aps.org/doi/10.1103/PhysRevResearch.6.013214 .
  • VanΒ OstenburgΒ etΒ al. [1962] D.Β O.Β VanΒ Ostenburg, D.Β J.Β Lam, H.Β D.Β Trapp,Β andΒ D.Β E.Β MacLeod,Β Knight Shifts and Magnetic Susceptibilities in V Alloys with Ti, Cr, and Tc,Β Phys. Rev.Β 128,Β 1550–1554 (1962),Β http://dx.doi.org/10.1103/PhysRev.128.1550 .
  • ShimizuΒ etΒ al. [1963] M.Β Shimizu, T.Β Takahashi,Β andΒ A.Β Katsuki,Β Magnetic susceptibility and electronic specific heat of transition metals and alloys iv. V and Ti metals and V-Cr and V-Ti alloys,Β J. Phys. Soc. JpnΒ 18,Β 1192–1203 (1963),Β http://dx.doi.org/10.1143/JPSJ.18.1192 .
  • Drain [1964] L.Β E.Β Drain,Β The temperature dependence of the nuclear magnetic resonance of vanadium,Β P. Phys. Soc.Β 83,Β 755–762 (1964),Β http://dx.doi.org/10.1088/0370-1328/83/5/307 .
  • CLOGSTONΒ etΒ al. [1964] A.Β M.Β CLOGSTON, A.Β C.Β GOSSARD, V.Β JACCARINO,Β andΒ Y.Β YAFET,Β Orbital Paramagnetism and the Knight Shift in Transition Metal Superconductors,Β Rev. Mod. Phys.Β 36,Β 170–175 (1964),Β http://dx.doi.org/10.1103/RevModPhys.36.170 .
  • TsudaΒ etΒ al. [1983] T.Β Tsuda, H.Β Yasuoka, Y.Β Kitaoka,Β andΒ F.Β DiΒ Salvo,Β 51V NMR study of the phase transition in 1T-VS2,Β J. Magn. Magn. Mater.Β 31–34,Β 1101–1102 (1983),Β http://dx.doi.org/10.1016/0304-8853(83)90816-8 .
  • BoutinΒ etΒ al. [2016] S.Β Boutin, J.Β RamΓ­rez-Ruiz,Β andΒ I.Β Garate,Β Tight-binding theory of NMR shifts in topological insulators Bi2⁒Se3subscriptBi2subscriptSe3{\mathrm{Bi}}_{2}{\mathrm{Se}}_{3}roman_Bi start_POSTSUBSCRIPT 2 end_POSTSUBSCRIPT roman_Se start_POSTSUBSCRIPT 3 end_POSTSUBSCRIPT and Bi2⁒Te3subscriptBi2subscriptTe3{\mathrm{Bi}}_{2}{\mathrm{Te}}_{3}roman_Bi start_POSTSUBSCRIPT 2 end_POSTSUBSCRIPT roman_Te start_POSTSUBSCRIPT 3 end_POSTSUBSCRIPT,Β Phys. Rev. BΒ 94,Β 115204 (2016),Β https://link.aps.org/doi/10.1103/PhysRevB.94.115204 .
  • MozaffariΒ etΒ al. [2023] S.Β Mozaffari, W.Β R.Β Meier, R.Β P.Β Madhogaria, S.-H.Β Kang, J.Β W.Β Villanova, H.Β W.Β S.Β Arachchige, G.Β Zheng, Y.Β Zhu, K.-W.Β Chen, K.Β Jenkins, etΒ al.,Β Universal sublinear resistivity in vanadium kagome materials hosting charge density waves,Β arXiv preprint arXiv:2305.02393Β  (2023).
  • HarrisΒ etΒ al. [2008] R.Β K.Β Harris, E.Β D.Β Becker, S.Β M.Β C.Β DeΒ Menezes, P.Β Granger, R.Β E.Β Hoffman,Β andΒ K.Β W.Β Zilm,Β Further Conventions for NMR Shielding and Chemical Shifts (IUPAC Recommendations 2008),Β Magn. Reson. Chem.Β 46,Β 582 (2008),Β https://doi.org/10.1002/mrc.2225 .
  • PerdewΒ etΒ al. [1996] J.Β P.Β Perdew, K.Β Burke,Β andΒ M.Β Ernzerhof,Β Generalized-gradient approximation made simple,Β Phys. Rev. Lett.Β 77,Β 3865 (1996),Β 0927-0256(96)00008 .

SUPPLEMENTARY INFORMATION:
Orbital selective commensurate modulations of the local density of states in ScV6⁒Sn6subscriptScV6subscriptSn6\textrm{ScV}_{6}\textrm{Sn}_{6}ScV start_POSTSUBSCRIPT 6 end_POSTSUBSCRIPT Sn start_POSTSUBSCRIPT 6 end_POSTSUBSCRIPT probed by nuclear spins

R. Guehne,1 J. Noky,1 C. Yi,1 C. Shekhar,1 M. G. Vergniory,1,2 M. Baenitz,1 and C. Felser1
1Max Planck Institute for Chemical Physics of Solids, 01187, Dresden, Germany
2Donostia International Physics Center, 20018 Donostia - San Sebastian, Spain

The following supplement comprises additional experimental data that constitutes essential complementary evidence to the already documented results which did not make it into the main file for reason of space. We will first present temperature dependent spectra for the cβˆ₯B0conditional𝑐subscript𝐡0c\parallel B_{0}italic_c βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT orientation, detailed orientation dependent NMR spectra that allows us to evaluate the electric field gradient (EFG) at the V nuclei for high and low temperatures, as well as the NMR shift anisotropy. We will next show how the NMR shift is extracted for the aβˆ—βˆ₯B0conditionalsuperscriptπ‘Žβˆ—subscript𝐡0a^{\ast}\parallel B_{0}italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT spectrum where the central transitions are hidden. We will then provide evidence that the total signal intensity can be brought into consistent agreement with changes in temperature, circuit performance, and rf-penetration depth. We will further provide some field dependent measurements, as well as a detailed analysis of the high temperature spin-lattice relaxation to conclude on its magnetic origin.

Appendix A Temperature dependent 51V spectra for cβˆ₯B0conditional𝑐subscript𝐡0c\parallel B_{0}italic_c βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT

In Fig.Β 7 we show a detailed account of the spectral changes for temperatures between 170Β times170absent170\text{\,}start_ARG 170 end_ARG start_ARG times end_ARG start_ARG end_ARG and 20Β Ktimes20K20\text{\,}\mathrm{K}start_ARG 20 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG and cβˆ₯B0conditional𝑐subscript𝐡0c\parallel B_{0}italic_c βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT. The highlighted range of temperatures denotes the CDW phase transition where the high temperature spectrum is progressively replaced by the 3 low temperature spectra.

Refer to caption
Figure 7: Temperature dependent 51V NMR spectra for cβˆ₯B0conditional𝑐subscript𝐡0c\parallel B_{0}italic_c βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT and 8.73Β Ttimes8.73T8.73\text{\,}\mathrm{T}start_ARG 8.73 end_ARG start_ARG times end_ARG start_ARG roman_T end_ARG (combined Fourier transformed selective spin echoes). The highlighted temperature range marks the phase transition. The peculiar low temperature intensity pattern, especially the pronounced first high frequency satellite, reveal changes in the NMR shift in addition to the obvious differences in the quadrupole splitting frequencies.

Appendix B Evaluation of the EFG tensor at high and low temperatures

In the following Figures 8 to 11 the results of detailed orientation dependent measurements are provided. The experiments were carried out for 170Β Ktimes170K170\text{\,}\mathrm{K}start_ARG 170 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG (Figs.Β 8 to 10) and 80Β Ktimes80K80\text{\,}\mathrm{K}start_ARG 80 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG (Fig.Β 11) at a magnetic field at 8.73Β Ttimes8.73T8.73\text{\,}\mathrm{T}start_ARG 8.73 end_ARG start_ARG times end_ARG start_ARG roman_T end_ARG using broad band FIDs (0.5 μ⁒stimes0.5πœ‡s0.5\text{\,}\mu\mathrm{s}start_ARG 0.5 end_ARG start_ARG times end_ARG start_ARG italic_ΞΌ roman_s end_ARG) and stepwise rotation of the single crystal placed on a single axis goniometer. When rotating the EFG about one of its principle axis (X,Yπ‘‹π‘ŒX,Yitalic_X , italic_Y or Z𝑍Zitalic_Z) the apparent quadrupole splitting Ξ½~Qsubscript~πœˆπ‘„\tilde{\nu}_{Q}over~ start_ARG italic_Ξ½ end_ARG start_POSTSUBSCRIPT italic_Q end_POSTSUBSCRIPT of the observed spectrum changes according to

Ξ½~Q=Ξ½Q2⁒(3⁒cos2β‘Ξ²βˆ’1+η⁒sin2⁑β⁒cos⁑2⁒α)subscript~πœˆπ‘„subscriptπœˆπ‘„23superscript2𝛽1πœ‚superscript2𝛽2𝛼\tilde{\nu}_{Q}=\frac{\nu_{Q}}{2}(3\cos^{2}\beta-1+\eta\sin^{2}\beta\cos 2\alpha)over~ start_ARG italic_Ξ½ end_ARG start_POSTSUBSCRIPT italic_Q end_POSTSUBSCRIPT = divide start_ARG italic_Ξ½ start_POSTSUBSCRIPT italic_Q end_POSTSUBSCRIPT end_ARG start_ARG 2 end_ARG ( 3 roman_cos start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT italic_Ξ² - 1 + italic_Ξ· roman_sin start_POSTSUPERSCRIPT 2 end_POSTSUPERSCRIPT italic_Ξ² roman_cos 2 italic_Ξ± ) (6)

where Ξ½Qsubscriptπœˆπ‘„\nu_{Q}italic_Ξ½ start_POSTSUBSCRIPT italic_Q end_POSTSUBSCRIPT denotes the quadrupole splitting frequency defined in the main text and α𝛼\alphaitalic_Ξ± and β𝛽\betaitalic_Ξ² are the Euler angles in the PAS of the EFGs.

Note, the various orientation dependent measurements are carried out to consistently determine the orientation of the EFG with respect to the lattice. Size (VZ⁒Zsubscript𝑉𝑍𝑍V_{ZZ}italic_V start_POSTSUBSCRIPT italic_Z italic_Z end_POSTSUBSCRIPT) and shape (Ξ·πœ‚\etaitalic_Ξ·) are obtained from measurements with the single crystal being well adjusted along the Z𝑍Zitalic_Z and Yπ‘ŒYitalic_Y direction and making use of the EFG being traceless and the definition of the asymmetry parameter.

Refer to caption
Figure 8: Orientation dependent broad band NMR spectra at 170Β Ktimes170K170\text{\,}\mathrm{K}start_ARG 170 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG and 8.73Β Ttimes8.73T8.73\text{\,}\mathrm{T}start_ARG 8.73 end_ARG start_ARG times end_ARG start_ARG roman_T end_ARG for crystal rotations around the crystal b𝑏bitalic_b-axis which corresponds to a rotation about the X𝑋Xitalic_X-axis of the EFG’s PAS (gray ellipsoid). Thus, the rotation connects VZ⁒Zsubscript𝑉𝑍𝑍V_{ZZ}italic_V start_POSTSUBSCRIPT italic_Z italic_Z end_POSTSUBSCRIPT and VY⁒Ysubscriptπ‘‰π‘Œπ‘ŒV_{YY}italic_V start_POSTSUBSCRIPT italic_Y italic_Y end_POSTSUBSCRIPT. Note, only the black resonances belong to this well defined rotation, while unmarked resonances represent the other two V nuclei per V triangle that undergo a rotation that leaves the PAS and can thus only be evaluated with much more difficulty. In addition, just above 97Β MHztimes97MHz97\text{\,}\mathrm{M}\mathrm{H}\mathrm{z}start_ARG 97 end_ARG start_ARG times end_ARG start_ARG roman_MHz end_ARG and at about 98.75Β MHztimes98.75MHz98.75\text{\,}\mathrm{M}\mathrm{H}\mathrm{z}start_ARG 98.75 end_ARG start_ARG times end_ARG start_ARG roman_MHz end_ARG the isotropic 27Al (light green) and 63Cu (light red) resonance lines, respectively, can be seen. The signal stem from a small piece of Al metal inside, and from the Cu wire of the rf-coil. The plot on the right hand side shows the quadrupole splitting as function of angle, including the typical fit using the formula above and keeping Ξ±=90 °𝛼times90degree\alpha=$90\text{\,}\mathrm{\SIUnitSymbolDegree}$italic_Ξ± = start_ARG 90 end_ARG start_ARG times end_ARG start_ARG Β° end_ARG.
Refer to caption
Figure 9: Orientation dependent broad band NMR spectra at 170Β Ktimes170K170\text{\,}\mathrm{K}start_ARG 170 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG and 8.73Β Ttimes8.73T8.73\text{\,}\mathrm{T}start_ARG 8.73 end_ARG start_ARG times end_ARG start_ARG roman_T end_ARG for crystal rotations around the crystal c𝑐citalic_c-axis which corresponds to a rotation about the Yπ‘ŒYitalic_Y-axis of the EFG’s PAS (gray ellipsoid). Thus, the rotation connects VZ⁒Zsubscript𝑉𝑍𝑍V_{ZZ}italic_V start_POSTSUBSCRIPT italic_Z italic_Z end_POSTSUBSCRIPT and VX⁒Xsubscript𝑉𝑋𝑋V_{XX}italic_V start_POSTSUBSCRIPT italic_X italic_X end_POSTSUBSCRIPT, the values of which are easily extracted. Note, since the PAS of the EFG’s of each of the three V nuclei per V triangle share the Z𝑍Zitalic_Z-axis, all of the resonances (black, blue, and red) can be used to evaluate the EFGs as shown in the plot on the right hand side. Again, the isotropic 27Al and 63Cu resonance lines are visible. This time, Ξ±=0 °𝛼times0degree\alpha=$0\text{\,}\mathrm{\SIUnitSymbolDegree}$italic_Ξ± = start_ARG 0 end_ARG start_ARG times end_ARG start_ARG Β° end_ARG and the phase shift dβ‰ˆΒ±60 °𝑑plus-or-minustimes60degreed\approx\pm$60\text{\,}\mathrm{\SIUnitSymbolDegree}$italic_d β‰ˆ Β± start_ARG 60 end_ARG start_ARG times end_ARG start_ARG Β° end_ARG determines the relative orientation of the three EFG’s and the sixfold symmetry of the Kagome lattice.
Refer to caption
Figure 10: Orientation dependent broad band NMR spectra at 170Β Ktimes170K170\text{\,}\mathrm{K}start_ARG 170 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG and 8.73Β Ttimes8.73T8.73\text{\,}\mathrm{T}start_ARG 8.73 end_ARG start_ARG times end_ARG start_ARG roman_T end_ARG for crystal rotations around the crystal aβˆ—superscriptπ‘Žβˆ—a^{\ast}italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT-axis which corresponds to a rotation about the Z𝑍Zitalic_Z-axis of the EFG’s PAS (gray ellipsoid). Thus, the rotation connects VY⁒Ysubscriptπ‘‰π‘Œπ‘ŒV_{YY}italic_V start_POSTSUBSCRIPT italic_Y italic_Y end_POSTSUBSCRIPT and VX⁒Xsubscript𝑉𝑋𝑋V_{XX}italic_V start_POSTSUBSCRIPT italic_X italic_X end_POSTSUBSCRIPT. Note, only the black resonances belong to this well defined rotation, while unmarked resonances belong to the other two V nuclei per V triangle that undergo a rotation that leaves their PAS and can thus only be evaluated with much more difficulty. The plot on the right hand side shows the quadrupole splitting as function of angle, including the typical fit using the formula above while keeping Ξ²=90 °𝛽times90degree\beta=$90\text{\,}\mathrm{\SIUnitSymbolDegree}$italic_Ξ² = start_ARG 90 end_ARG start_ARG times end_ARG start_ARG Β° end_ARG.
Refer to caption
Figure 11: Orientation dependent broad band NMR spectra at 80Β Ktimes80K80\text{\,}\mathrm{K}start_ARG 80 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG and 8.73Β Ttimes8.73T8.73\text{\,}\mathrm{T}start_ARG 8.73 end_ARG start_ARG times end_ARG start_ARG roman_T end_ARG for crystal rotations around the crystal c𝑐citalic_c-axis similar to the one shown in Fig.Β 9. In the CDW phase, the NMR spectrum visible splits into 3 individual spectra for each of the 3 V per V triangle (green, red, and blue βˆ’-- in light, regular, and dark color) while the sixfold symmetry of the Kagome lattice is retained. The plot on the right documents the orientation dependence and sixfold symmetry of the underlaying lattice.

Appendix C Determination of the NMR shift for the in-plane orientation

For cβˆ₯B0conditional𝑐subscript𝐡0c\parallel B_{0}italic_c βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT the central transitions and thus the NMR shift are directly accessible as can be seen in Fig.Β 4 (A). For the aβˆ—βˆ₯B0conditionalsuperscriptπ‘Žβˆ—subscript𝐡0a^{\ast}\parallel B_{0}italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT orientation, the CTs (for high and low temperatures) are hidden behind the broad quadrupole spectrum of the 2 other V nuclei in each V triangle. In order to obtain the NMR shift, therefore, the satellites can be used, and the first order (equidistant) quadrupole pattern. The procedure is shown in Fig.Β 12. The relevant low temperature spectrum consists of 3 equally intense quadrupole patterns differing in shift and quarupole splitting (purple, orange, and light blue).

Refer to caption
Figure 12: Fourier transform of a broad band NMR signal for 80Β Ktimes80K80\text{\,}\mathrm{K}start_ARG 80 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG and 8.73Β Ttimes8.73T8.73\text{\,}\mathrm{T}start_ARG 8.73 end_ARG start_ARG times end_ARG start_ARG roman_T end_ARG with the single crystal aligned as aβˆ—βˆ₯B0conditionalsuperscriptπ‘Žβˆ—subscript𝐡0a^{\ast}\parallel B_{0}italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT. The four spectra below represent the three individual quadrupole patterns (colored) and their sum (black).

Appendix D NMR shift anisotropy

For the high temperatures, the NMR shift was found to be axially symmetric, as there is essentially no change in the resonance frequency of the CT in Fig.Β 10. It is a reasonable assumption that the CDW phase inherits this symmetry. The corresponding isotropic (Kiso=(2⁒Kc+Kaβˆ—)/3subscript𝐾iso2subscript𝐾𝑐subscript𝐾superscriptπ‘Žβˆ—3K_{\mathrm{iso}}=(2K_{c}+K_{a^{\ast}})/3italic_K start_POSTSUBSCRIPT roman_iso end_POSTSUBSCRIPT = ( 2 italic_K start_POSTSUBSCRIPT italic_c end_POSTSUBSCRIPT + italic_K start_POSTSUBSCRIPT italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT end_POSTSUBSCRIPT ) / 3) and axial (Kaxial=2⁒(Kcβˆ’Kaβˆ—)/3subscript𝐾axial2subscript𝐾𝑐subscript𝐾superscriptπ‘Žβˆ—3K_{\mathrm{axial}}=2(K_{c}-K_{a^{\ast}})/3italic_K start_POSTSUBSCRIPT roman_axial end_POSTSUBSCRIPT = 2 ( italic_K start_POSTSUBSCRIPT italic_c end_POSTSUBSCRIPT - italic_K start_POSTSUBSCRIPT italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT end_POSTSUBSCRIPT ) / 3) shift components are shown in Fig.Β 13. The colors follow Fig.Β 4Β (C) and (D) and are identified with the high single temperature resonance V and three chemically non-equivalent low temperature V sites V1, V2, and V3. In the CDW phase, the isotropic shifts assume 3 different values, from about 0.743Β %times0.743percent0.743\text{\,}\%start_ARG 0.743 end_ARG start_ARG times end_ARG start_ARG % end_ARG for V1 to about 0.76Β %times0.76percent0.76\text{\,}\%start_ARG 0.76 end_ARG start_ARG times end_ARG start_ARG % end_ARG for V3. Surprisingly, their mean value (gray column in panel C) agrees almost exactly with Kisosubscript𝐾isoK_{\mathrm{iso}}italic_K start_POSTSUBSCRIPT roman_iso end_POSTSUBSCRIPT for the high temperature resonance just above the onset of CDW phase transition at 96Β Ktimes96K96\text{\,}\mathrm{K}start_ARG 96 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG (black column). Contrastingly, the anisotropy of all 3 low temperature V sites increases, yielding values between βˆ’0.14Β %times-0.14percent-0.14\text{\,}\%start_ARG - 0.14 end_ARG start_ARG times end_ARG start_ARG % end_ARG (V3) to almost βˆ’0.17Β %times-0.17percent-0.17\text{\,}\%start_ARG - 0.17 end_ARG start_ARG times end_ARG start_ARG % end_ARG (V2). The mean axial shift component (gray) deviates clearly from the high temperature Kaxialsubscript𝐾axialK_{\mathrm{axial}}italic_K start_POSTSUBSCRIPT roman_axial end_POSTSUBSCRIPT at 96Β Ktimes96K96\text{\,}\mathrm{K}start_ARG 96 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG, with a difference in the order of 190Β ppmtimes190ppm190\text{\,}\mathrm{p}\mathrm{p}\mathrm{m}start_ARG 190 end_ARG start_ARG times end_ARG start_ARG roman_ppm end_ARG (0.019Β %times0.019percent0.019\text{\,}\%start_ARG 0.019 end_ARG start_ARG times end_ARG start_ARG % end_ARG). Thus, one way to look at the CDW transition is through the shift anisotropy, with a net change in the axial part of the shift (Δ⁒KaxialΞ”subscript𝐾axial\Delta K_{\mathrm{axial}}roman_Ξ” italic_K start_POSTSUBSCRIPT roman_axial end_POSTSUBSCRIPT), while the average isotropic shift remains unaltered in comparison to the high temperature phase.

Refer to caption
Figure 13: The isotropic and axial shift component as functions of temperature. Note that for low temperatures an axial symmetry cannot be verified with the experiment. The values during the phase transition are missing because for aβˆ—βˆ₯B0conditionalsuperscriptπ‘Žβˆ—subscript𝐡0a^{\ast}\parallel B_{0}italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT it is not possible to identify individual resonances due to the overlap of resonances.

Appendix E The circuit’s quality factor, rf-penetration depth, and the total signal intensity

Refer to caption
Figure 14: (A) The CT for cβˆ₯B0conditional𝑐subscript𝐡0c\parallel B_{0}italic_c βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT as a function of temperature reproduced from Fig.Β 4. The gray areas correspond to the total signal intensity. (B) The rf-circuit’s quality factor Q𝑄Qitalic_Q as a function of temperature. Clearly, a bend in the dependence is visible at the onset of the CDW phase transition, most potentially due to the corresponding change in the sample resistivity and the thus changing rf-penetration depth that affects the inductance of the rf-coil. (C The CT signal intensity from panel (A) after correction for the temperature and Q𝑄Qitalic_Q fits matches almost perfectly with the T𝑇Titalic_T dependence of the rf-penetration depth (rescaled to match the 100Β Ktimes100K100\text{\,}\mathrm{K}start_ARG 100 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG value of the intensity) implying the loss in signal intensity is due to a loss in accessible nuclei from a reduced penetration depth.

To evaluate the total signal intensity we investigate the central transition of Fig.Β 4 (A). This allows us to eliminate some uncertainties that are connected with the excitation conditions in terms of selective excitations, power levels, band widths etc. The CTs are nevertheless representative for the total signal intensity. We reproduce the spectra in Fig.Β 14 (A). These spectra are corrected for signal averaging as well as for the temperature. An NMR signal is further proportional to Q𝑄\sqrt{Q}square-root start_ARG italic_Q end_ARG, where Q𝑄Qitalic_Q is the quality factor of the rf-circuit. We plot Q𝑄Qitalic_Q as a function of temperature in panel (B). Q𝑄Qitalic_Q changes with temperature since it is connected to the resistivity of the sample. We thus corrected the signal intensity given by the gray area under the curves in panel (A) by the changes in Q𝑄Qitalic_Q, and plot it in panel (C) as gray stars. Finally, since the resistivity of the sample changes significantly as a function of temperature [15], we estimated the corresponding penetration depth of the rf-field at f=100Β MHz𝑓times100MHzf=$100\text{\,}\mathrm{M}\mathrm{H}\mathrm{z}$italic_f = start_ARG 100 end_ARG start_ARG times end_ARG start_ARG roman_MHz end_ARG due to the skin effect, using δ⁒(T)=2⁒ρ⁒(T)/(2⁒π⁒f⁒μ0)𝛿𝑇2πœŒπ‘‡2πœ‹π‘“subscriptπœ‡0\delta(T)=\sqrt{2\rho(T)/(2\pi f\mu_{0})}italic_Ξ΄ ( italic_T ) = square-root start_ARG 2 italic_ρ ( italic_T ) / ( 2 italic_Ο€ italic_f italic_ΞΌ start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT ) end_ARG, where ρ𝜌\rhoitalic_ρ denotes the sample resistivity, f𝑓fitalic_f the frequency, and ΞΌ0subscriptπœ‡0\mu_{0}italic_ΞΌ start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT the vacuum magnetic permeability. The results are plotted as purple triangles in panel (C). Consistently, as the resistivity decreases with decreasing temperature, the skin depth decreases as well, thus, reducing the number of nuclear accessible with NMR. Obviously, the total signal intensity’s dependence on temperature follows very well the changes of the skin depth expected for a thick sample (200 μ⁒mtimes200πœ‡m200\text{\,}\mu\mathrm{m}start_ARG 200 end_ARG start_ARG times end_ARG start_ARG italic_ΞΌ roman_m end_ARG). This analysis confirms that we have no unusual intensity loss in the present system.

Refer to caption
Figure 15: Fourier transform of spin-echo measurements of the central double-peak for cβˆ₯B0conditional𝑐subscript𝐡0c\parallel B_{0}italic_c βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT and 50Β Ktimes50K50\text{\,}\mathrm{K}start_ARG 50 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG for external fields of 4.8, 6.7Β times6.7absent6.7\text{\,}start_ARG 6.7 end_ARG start_ARG times end_ARG start_ARG end_ARG, and 8.8Β Ttimes8.8T8.8\text{\,}\mathrm{T}start_ARG 8.8 end_ARG start_ARG times end_ARG start_ARG roman_T end_ARG in units of ppm. The red dashed lines denote the approximate center frequencies of the two peaks. A constant splitting in units of ppm proves the origin of the splitting is due to different NMR shifts (paramagnetic spin susceptibility) rather then an unusual magnetism.

Appendix F Magnetic field dependent measurements

The double-peak central transition structure from Fig. 4 (A) was measured for two more magnetic fields. The spectra are shown in Fig. 15 in units of ppm. Evidently, the two peaks do not change in relative position (150 ppmtimes150ppm150\text{\,}\mathrm{p}\mathrm{p}\mathrm{m}start_ARG 150 end_ARG start_ARG times end_ARG start_ARG roman_ppm end_ARG), nor in relative intensity. This is a strong evidence that the origin of this peak system is related to different Knight shift values, i.e., different DOS as expected from a CDW. Second order quadrupole effects (∝1/B0proportional-toabsent1subscript𝐡0\propto 1/B_{0}∝ 1 / italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT) obviously do not affect the spectrum, while, on the other hand, unusual magnetism as potentially related to orbital currents, are not evident.

Appendix G Magnetic relaxation and determination of T1subscript𝑇1T_{1}italic_T start_POSTSUBSCRIPT 1 end_POSTSUBSCRIPT

In a quadrupolar split system, it can be difficult to determine T1subscript𝑇1T_{1}italic_T start_POSTSUBSCRIPT 1 end_POSTSUBSCRIPT, as it is defined to be the relaxation time of the unsplit spin system, i.e., as if no quadrupole interaction is present. For 51V, the quadrupole spectrum covers almost 3Β MHztimes3MHz3\text{\,}\mathrm{M}\mathrm{H}\mathrm{z}start_ARG 3 end_ARG start_ARG times end_ARG start_ARG roman_MHz end_ARG and thus, the relaxation of individual transitions is the only way to measure T1subscript𝑇1T_{1}italic_T start_POSTSUBSCRIPT 1 end_POSTSUBSCRIPT for fairly well defined conditions. The relaxation of individual transition, however, depends on the transition and the relaxation mechanism, i.e., whether its driven by magnetic fluctuations due to free carriers or lattice vibrations via the quadrupole interaction.

In order to check the relaxation mechanism in the current system, we assume the relaxation to be of magnetic origin, and apply the corresponding recovery equations to extract T1subscript𝑇1T_{1}italic_T start_POSTSUBSCRIPT 1 end_POSTSUBSCRIPT. We used selective saturation recovery pulse sequences and analyzed the individual recovery curves with:

M⁒(t)=M0⁒[1βˆ’f⁒{βˆ‘i=17aiβ‹…exp⁑(βˆ’Ξ»i⁒tT1)}],𝑀𝑑subscript𝑀0delimited-[]1𝑓superscriptsubscript𝑖17β‹…subscriptπ‘Žπ‘–subscriptπœ†π‘–π‘‘subscript𝑇1M(t)=M_{0}\left[1-f\Biggl{\{}\sum_{i=1}^{7}a_{i}\cdot\exp\left(-\frac{\lambda_% {i}t}{T_{1}}\right)\Biggr{\}}\right]\ ,italic_M ( italic_t ) = italic_M start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT [ 1 - italic_f { βˆ‘ start_POSTSUBSCRIPT italic_i = 1 end_POSTSUBSCRIPT start_POSTSUPERSCRIPT 7 end_POSTSUPERSCRIPT italic_a start_POSTSUBSCRIPT italic_i end_POSTSUBSCRIPT β‹… roman_exp ( - divide start_ARG italic_Ξ» start_POSTSUBSCRIPT italic_i end_POSTSUBSCRIPT italic_t end_ARG start_ARG italic_T start_POSTSUBSCRIPT 1 end_POSTSUBSCRIPT end_ARG ) } ] , (7)

where M0subscript𝑀0M_{0}italic_M start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT is the equilibrium signal intensity, and f𝑓fitalic_f the inversion factor (f=1𝑓1f=1italic_f = 1 saturation, f=2𝑓2f=2italic_f = 2 inversion). The coefficients aisubscriptπ‘Žπ‘–a_{i}italic_a start_POSTSUBSCRIPT italic_i end_POSTSUBSCRIPT vary for each transition, while the exponents Ξ»isubscriptπœ†π‘–\lambda_{i}italic_Ξ» start_POSTSUBSCRIPT italic_i end_POSTSUBSCRIPT are shared. We summarize the various values in Tab.Β 2.

Table 2: Coefficients aisubscriptπ‘Žπ‘–a_{i}italic_a start_POSTSUBSCRIPT italic_i end_POSTSUBSCRIPT and exponents Ξ»isubscriptπœ†π‘–\lambda_{i}italic_Ξ» start_POSTSUBSCRIPT italic_i end_POSTSUBSCRIPT for magnetic relaxation and recovery measurements of selectively saturated or inverted transitions of a spin 7/2727/27 / 2 system.
aisubscriptπ‘Žπ‘–a_{i}italic_a start_POSTSUBSCRIPT italic_i end_POSTSUBSCRIPT CT 1st Sat 2nd Sat 3rd Sat Ξ»1subscriptπœ†1\lambda_{1}italic_Ξ» start_POSTSUBSCRIPT 1 end_POSTSUBSCRIPT
i=1𝑖1i=1italic_i = 1 1/84 1/84 1/84 1/84 1
2 0 1/84 1/21 3/21 3
3 3/44 1/33 1/132 3/11 6
4 0 9/77 25/308 25/77 10
5 75/364 1/1092 100/273 75/364 15
6 0 49/132 49/132 3/44 21
7 1225/1716 392/858 98/858 8/858 28

The results are shown in Fig.Β 16. Black denotes the recovery for the CT, red for the first, petrol for the second, and pink for the third lower satellite. The results provide strong evidence for the assumption, because each of the 4 transition selective recoveries, i.e, CT and the three satellites, yield the same T1subscript𝑇1T_{1}italic_T start_POSTSUBSCRIPT 1 end_POSTSUBSCRIPT of 24⁒(1)Β mstimesuncertain241ms24(1)\text{\,}\mathrm{m}\mathrm{s}start_ARG start_ARG 24 end_ARG start_ARG ( 1 ) end_ARG end_ARG start_ARG times end_ARG start_ARG roman_ms end_ARG at 250Β Ktimes250K250\text{\,}\mathrm{K}start_ARG 250 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG and cβˆ₯B0conditional𝑐subscript𝐡0c\parallel B_{0}italic_c βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT. We further repeated the measurement for the 1st satellite at the same temperature for aβˆ—βˆ₯B0conditionalsuperscriptπ‘Žβˆ—subscript𝐡0a^{\ast}\parallel B_{0}italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT (blue data), which yields the same result, and hence, the relaxation is isotropic.

Finally, there are a few crystal orientations where one of the 3 V quadrupole splittings disappears, and therefore, the quadrupole interaction is eliminated. We used ∠⁒(c,B0)β‰ˆ75Β Β°βˆ π‘subscript𝐡0times75degree\angle(c,B_{0})\approx$75\text{\,}\mathrm{\SIUnitSymbolDegree}$∠ ( italic_c , italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT ) β‰ˆ start_ARG 75 end_ARG start_ARG times end_ARG start_ARG Β° end_ARG (cf. Fig.Β 8) to measure the pure T1subscript𝑇1T_{1}italic_T start_POSTSUBSCRIPT 1 end_POSTSUBSCRIPT of the un-split spin system (Fig.Β 16 yellow data) and applied the simple exponential relationship

M⁒(t)=M0⁒[1βˆ’fβ‹…exp⁑(βˆ’tT1)]𝑀𝑑subscript𝑀0delimited-[]1⋅𝑓𝑑subscript𝑇1M(t)=M_{0}\left[1-f\cdot\exp\left(-\frac{t}{T_{1}}\right)\right]italic_M ( italic_t ) = italic_M start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT [ 1 - italic_f β‹… roman_exp ( - divide start_ARG italic_t end_ARG start_ARG italic_T start_POSTSUBSCRIPT 1 end_POSTSUBSCRIPT end_ARG ) ] (8)

which, evidently, gives the same T1subscript𝑇1T_{1}italic_T start_POSTSUBSCRIPT 1 end_POSTSUBSCRIPT as for selective excitation in the other orientations. We have thus confirmed the relaxation to be driven by magnetic fluctuations from free electrons which is the prerequisite for our treatment of 1/T1⁒(T)1subscript𝑇1𝑇1/T_{1}(T)1 / italic_T start_POSTSUBSCRIPT 1 end_POSTSUBSCRIPT ( italic_T ) using the DOS.

Refer to caption
Figure 16: Evaluation of the spin-lattice relaxation at 250Β Ktimes250K250\text{\,}\mathrm{K}start_ARG 250 end_ARG start_ARG times end_ARG start_ARG roman_K end_ARG and 8.73Β Ttimes8.73T8.73\text{\,}\mathrm{T}start_ARG 8.73 end_ARG start_ARG times end_ARG start_ARG roman_T end_ARG. The plot shows the results from individual saturation recovery measurements carried out for the CT (black), and the first (red), second (petrol), and third (pink) satellite of the V spectrum for cβˆ₯B0conditional𝑐subscript𝐡0c\parallel B_{0}italic_c βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT, as well as for the first satellite (blue) for aβˆ—βˆ₯B0conditionalsuperscriptπ‘Žβˆ—subscript𝐡0a^{\ast}\parallel B_{0}italic_a start_POSTSUPERSCRIPT βˆ— end_POSTSUPERSCRIPT βˆ₯ italic_B start_POSTSUBSCRIPT 0 end_POSTSUBSCRIPT, and for the non-selective spectrum at 75Β Β°times75degree75\text{\,}\mathrm{\SIUnitSymbolDegree}start_ARG 75 end_ARG start_ARG times end_ARG start_ARG Β° end_ARG (yellow). The solid curves denote the best fit using equations (7), (8), and Tab.Β 2.