Introduction

Flexoelectricity is an emergent phenomenon that describes electric polarization controlled by inhomogeneous deformation, i.e., strain gradients, with broken inversion symmetry1,2. The flexoelectric effect has two basic features. One is its inherent universality, which allows the appearance of net polarization from strain gradients for every dielectric material, breaking the limit of piezoelectricity that merely exists in the piezoelectric materials of 20 noncentrosymmetric groups1,3. Second, when a given strain field is imposed, strain gradients and hence flexoelectricity are expected to be more considerable with the reduction of the spatial scale4,5. Therefore, the flexoelectric effect is pronounced at the nanoscale6,7,8,9 and has the potential to mediate local polar switching10,11, piezoelectric performance12,13, optoelectronic characteristics14, magnetic properties15,16, etc. In particular, dielectric oxides have a large flexoelectric coefficient and thus hold broad promise for application in future nanosized devices11,17. However, bending these brittle ceramic materials to realize appropriate and controllable strain gradients is difficult, hindering the achievement of a high flexoelectric response.

Grain boundaries (GBs), which consist of unique periodic arrangements of structural units, can exhibit different properties that are not present in intrinsic bulk crystals18,19,20,21,22. For a well-bonded symmetric GB, the atomic configuration of the GB core is a natural trapezoidal shape with a significantly inhomogeneous strain distribution in space. Such disrupted atomic bonding is usually confined to a few unit cells around the GB core, which is expected to introduce huge strain gradients23. In addition, tailoring the trapezoidal shape simply by controlling the orientations of two adjacent grains is predictable and practicable, resulting in an adjustable strain gradient as well as flexoelectric polarization. As a result, GBs may serve as a feasible component to realize remarkable and tunable nanoscale flexoelectricity. However, in practice, validating this speculation is challenging, as GBs are of atomic size and have complex structures, while conventional macroscopic characterizations and measurements only provide collective information about the bulk material and may be influenced by other irrelevant factors, such as surface effects24,25.

Here, we verify this speculation and develop a general strategy to generate atomic-scale flexoelectric polarization via GB engineering. For a 24° tilt LaAlO3 (LAO) GB, we directly visualize the atomic arrangements by advanced atomically resolved scanning transmission electron microscopy (STEM) and spectroscopy techniques and find a huge strain gradient (~1.2 nm−1) and a remarkable flexoelectric effect that induces atomic displacement up to 81.4 ± 10.5 pm within 3–4-unit cells around the GB. In such a confined GB region, a large local polarization (~38 μC cm−2, estimated by first-principles density functional theory (DFT) calculations) exists, forming a “head-to-head” polarization configuration. Electron energy loss spectroscopy (EELS) illustrates that the flexoelectric phase at the GB has stronger hybridization of La–O interactions. The presence of nanoscale flexoelectricity accompanied by a change in the electronic structures is expected to play a considerable role in the transport properties of electroceramics. Furthermore, when extrapolated to SrTiO3 (STO) GBs, huge strain gradients also exist in the 22.6° GB core, and even larger strain gradients are observed in the 36.8° GB, exhibiting that tunable flexoelectricity can be achieved by altering the misorientation angle of GBs in different materials. The demonstrated generality of atomic-scale flexoelectricity at GBs provides essential knowledge to understand the electrical activity of oxide ceramics. The tunability via GB engineering may open vistas in nanoelectronics and nanoelectromechanical systems.

Results

GB engineering design

Figure 1a shows the distinctive geometry of the GB in which huge strain gradients are achievable. Atoms in a symmetric tilt GB are confined by the perfect bulk matrix, subsequently forming periodic arrangements of trapezoidal structural units with large structural deformation, as highlighted in Fig. 1a. Generally, considerable flexoelectricity can only be obtained from significantly bent crystals2. In contrast, such an ideal atomic-sized trapezoid in the GB core is expected to generate a huge strain gradient and introduce a large dipole moment within a single unit cell. Based on the geometric relationship of the trapezoid-shaped unit (see “Methods” for details), we obtain the strain gradients in the GB core for different misorientation angles of the GB (Fig. 1b).

Fig. 1: Schematics of the design of a huge strain gradient via GB engineering.
figure 1

a Schematic of inhomogeneous deformation of the unit cell in a GB (flexoelectric coefficient f11 ≠ 0), producing a net dipole moment due to flexoelectricity (Pflexo). b Expected distribution of the strain gradient for different GB angles. The red dots represent experimental data from LAO and STO GBs. The error bar is the standard derivation.

Atomic-scale GB structure

Now, we verify the possible presence of flexoelectricity in such a structure by investigating a 24° tilt LAO GB. LAO has no known ferroelectric instability26 and is an insulating oxide typically used as a gate dielectric. The LAO bicrystal was fabricated by thermal diffusion bonding27,28, the correlative experimental details are presented in Methods. To pinpoint the atomic configurations and chemistries of the inhomogeneity, we employed various advanced STEM techniques. Figure 2a depicts the high-angle annular dark-field (HAADF) image (colored for clarity) viewed along the [001] direction, where structural units are periodically distributed along the [1\(\bar{5}\)0] projection highlighted by the dotted polygons. The brighter atom columns correspond to La columns, and the other atom type is Al, while the O columns are invisible due to the Z-contrast sensitivity of HAADF imaging. We, therefore, acquired an integrated differential phase contrast (iDPC) image (Fig. 2b), in which both cations and oxygen atoms are directly visible29. Combined with atomically resolved energy dispersive X-ray spectroscopy (EDS), which can be used to further check the possible chemical mixing in the GB (Fig. 2c), we ultimately determined the atomic arrangement in the buried GB, as schematically shown in Fig. 2d. Quantitative elemental analysis is also shown in Supplementary Fig. 1 to reveal the local chemistry across the GB, experimentally showing no distinguishable chemical intermixing or segregation. From the iDPC image, the oxygen octahedron distortions are recognizable at a few angstroms wide around the GB. The trapezoid-shaped units in the core structure of the GB impose huge strain gradients and lead to substantial distortion and shifts of AlO columns, intuitively visible to the naked eye.

Fig. 2: Atomic arrangements of the LAO GB.
figure 2

a HAADF image. The periodic structural units are highlighted by the white polygons. Scale bar, 1 nm. b iDPC image depicting the oxygen and cationic arrangement. Scale bar, 1 nm. c Atomically resolved EDS mapping to determine the cationic configuration in the GB. Magenta: La; cyan: Al. Scale bar, 1 nm. d Schematic representation of the complete atomic structure of the LAO GB illustrating structural distortion at the GB. Magenta: La; cyan: Al; purple: O.

Quantitative analysis of nanoscale flexoelectricity

To better characterize the flexoelectric effect at the GB, a map of atomic displacements was extracted based on the iDPC image, as illustrated in Fig. 3a, wherein the overlaid vectors represent the magnitude and direction of the AlO column offsets with respect to the center of the surrounding four La columns. Such a cationic displacement measurement can minimize the tilt effect30, which is inevitable for GB measurement, as the two grains are not exactly identical in terms of zone axes (see details in the Methods and Supplementary Fig. 2). A “head-to-head” configuration pattern of polar vectors emerges around the GB. Note that the magnitude of these vectors is typically higher than the level of noise and possible artifacts (see details in the “Methods” section). To further evaluate the flexoelectric performance of the GB, we quantitatively mapped the strain and strain gradient based on the cation sublattices in the iDPC image (Fig. 3b–e). The surrounding grains away from the GB were regarded as the reference of a perfect (unstrained) crystal. The strength of the strain parallel to the GB plane (exx) is small (Fig. 3c), while the strain gradients from ezz along the horizontal (d(ezz)/dz in Fig. 3d) and vertical (d(ezz)/dx in Fig. 3e) directions are noticeable within 1 unit cell away from the structural unit. Such a highly nonuniform strain distribution around the GB core is also verified by the geometric phase analysis (GPA) in Supplementary Fig. 331. In particular, the unique core structure of the GB (marked by the red trapezoid in Figs. 3a and 4a) undergoes drastic fluctuation of the strain gradient up to 1.2 nm−1 (d(ezz)/dx), producing a significant polar displacement (~81.4 ± 10.5 pm) which is expected to generate large flexoelectric polarization (more details on error estimation are included in the “Methods” section), while the strain gradients d(ezz)/dz are negligible due to the symmetric geometry along this direction. For the shear strain, its contribution to the overall flexoelectricity should be very small according to previous theoretical studies32.

Fig. 3: Atomic-scale displacements and strain gradients in the LAO GB.
figure 3

a Off-center displacement vector map between the La and AlO columns from the iDPC image. The structural units of the GB are highlighted by the white polygons. The arrows represent the magnitude and direction of polar displacements estimated based on the offsets of the AlO column with respect to the center of the surrounding four La columns. Scale bar, 1 nm. b, c Unit cell-scale mapping of ezz (b) and exx (c) corresponding to the strain perpendicular and parallel to the GB plane, respectively. Scale bar, 1 nm. d, e Strength of the strain gradients from ezz. d, e Horizontal (d(ezz)/dz) and vertical (d(ezz)/dx) strain gradients, respectively. The structural units of the GB are highlighted by the white polygons. Scale bar, 1 nm.

Fig. 4: Polarization and electronic structures of the LAO GB.
figure 4

a Atomic structure and polarization of the GB from DFT calculations. Vectors denote the polarization direction for each unit cell. The strength of polarization is expressed as a color map, ranging from white (weak) to yellow (strong). In the red polyhedron, the displacement between the cations and oxygen atoms in the AlO octahedron is clearly visible with an upward component, accounting for the deviation between the polar vector and displacement vector. b O K-edges from the GB core (red) and grains (blue) indicating stronger hybridization of La–O interactions in the GB. c Al L-edges and La N-edges manifesting different local Al–O configurations in the GB. The corresponding Al L3 (yellow) and L2 (green)-edges are marked for clarity. d Calculated density of states of the GB core (red) and grains (blue). The valence band maximum (VBM) energies in the bulk and at the GB are set to zero.

Based on the DFT calculation in Fig. 4a, the maximum polarization of this trapezoidal-shaped unit is evaluated as ~38 μC cm−2. The longitudinal flexoelectric coefficient f11 of LAO can then be estimated as 0.3 nC m−1, manifesting reasonable agreement with the values in a previous work obtained from theoretical calculations of similar materials25. Despite the small difference due to the complex environment of the GB core, the overall atomic structure in the GB presented by DFT calculations is in decent agreement with the experimental results, as illustrated in Supplementary Fig. 4. Hence, the simple consideration of the off-centering between cationic columns delivers the main features of the polar vector distribution, except for the red polyhedron in Figs. 3a and 4a, in which the calculation shows that the displacement between the cations and oxygen atoms in the AlO octahedron has an upward component and dominates the polar vector, causing a discrepancy with the experimental cationic displacement results. Interestingly, the polarizations around the GB also point toward the GB core, forming a “head-to-head” configuration with an average value of ~10 μC cm−2 from each grain side, analogous to the charged domain wall in ferroelectrics. Furthermore, the charge density distribution calculated by DFT simulations (Supplementary Fig. 5a) shows that electrons have a sharp maximum value at the GB, which can effectively screen the depolarizing fields and stabilize the head-to-head polarization configurations. Moreover, four-dimensional STEM (4D-STEM) measurements (see details in the “Methods” section) in Supplementary Fig. 5b–d further validate the presence of negative charge accumulation at the GB, which certainly plays an important role in determining the electrical activities of the GB in these electroceramics.

Electrical structure of the GB

Therefore, we performed EELS at the oxygen K-edge and the aluminum L-edge to investigate the electronic structure of the flexoelectric phase in the GB. For reliability and accuracy of the data, we carefully chose clean and uniform regions to perform EELS measurements, as shown in Supplementary Fig. 6 (see details in the “Methods” section). The spectra from the bulk matrix and the GB core are extracted in Fig. 4b, c. The oxygen K-edge spectra (Fig. 4b) illustrate a similar peak at 536.5 eV in the bulk and GB core, which is related to La 5d–O 2p hybridized states33, while a feature at approximately 533.5 eV (peak A) only exists in the GB, indicating stronger La–O interactions34. Spectral region B corresponds to the transition to O 2p states hybridized with Al 3p states34,35. The different fine structure of spectral region B in the GB demonstrates the modified hybridization between Al and O states. A previous study reported that the hybridization between Ti 3d and O 2p in PbTiO3 and BaTiO3 accounts for their ferroelectricity36. Therefore, the stronger La–O hybridization in the GB core is in well agreement with the presence of flexoelectricity. Additionally, the Al L-edge spectrum generally exhibits a fingerprint that signifies the change in the Al coordination symmetry and reflects the unoccupied conduction band minimum (CBM)37,38,39. As shown in Fig. 4c, the decrease in the threshold energy at the Al L3-edge highlighted by the arrow is ~0.6 eV, illustrating distorted octahedral symmetry in the GB area40, which is also reflected in the difference in the fine structure at the Al L1-edge (Supplementary Fig. 7a)41 and the substantial reduction in the L3/L2 ratio (depicted in Supplementary Fig. 7b). Furthermore, because the Al L2,3-edges originate from the electron excitations from the Al 2p to unoccupied Al 3s states, while the Al 3s orbital dominates the CBM39, the lower onset energy may also manifest a band gap reduction in the GB, which is confirmed by DFT calculations of the density of states (Fig. 4d) and electronic band structure (Supplementary Fig. 8).

Discussion

To validate the generality of the flexoelectricity in the GB, we then investigated SrTiO3 (STO) GBs to present the universal structural information associated with adjustable flexoelectricity. As shown in Supplementary Fig. 9, the maximum strain gradient in the 22.6° STO GB is evaluated as ~1.5 nm−1 for d(ezz)/dx, resulting in a cationic atomic shift of up to 60.3 ± 5.7 pm. The strain gradients are more pronounced in the 36.8° STO GB core (~1.9 nm−1 for d(ezz)/dx), inducing giant atomic shifts up to ~119.1 ± 4.3 pm (Supplementary Fig. 10). Note that such an enhancement of displacements might not only be caused by flexoelectricity but also partly come from the nonstoichiometry which are usually strongly coupled with each other23. We also measured the EELS spectra for different STO GBs, and found them very different. For example, the 22.6° STO GB shows more decreased crystal field splitting (Supplementary Fig. 11). However, it should also be noted that in addition to the flexoelectricity, the electrical changes in the GB are probably influenced by multiple factors, such as bonding changes, possible local charge changes, and their interactions, rather than only flexoelectricity. On the other hand, the strain gradients in the LAO and STO GB cores measured by experiments (depicted in Fig. 1b and highlighted by red dots), show good consistency with the estimated geometric relation, indicating that a wide range of strain gradients can be obtained by controlling the GB angle. In addition to tunability and universality, GB engineering has advantages in generating flexoelectricity compared with other strategies, such as changing the epitaxial conditions or other defects. For example, although great tensile strains exist in the center of cracks in STO42, symmetric stretching prevents the flexoelectric polarization response due to the small strain gradients. In contrast, the GB restricts the large strain gradients to within a few unit cells, serving to deterministically trigger nanoscale flexoelectricity.

Moreover, the polarized GB core further influences the electrostatic potential and the electronic density in the GB, modulating the electrical activities. Taking LAO as an example, a stronger hybridization state is located in the GB core, favoring and promoting the formation of polar distortion. The decrease in the Al L3 onset energy indicates disordered configuration complexity, which may allow weak p–d hybridized states that are forbidden in the perfect AlO6 octahedral configuration, possibly causing a small number of defective states between the valence band maximum (VBM) and CBM39,40. In addition, around the GB, the flexoelectric distortion may also couple with the rotational distortion (e.g., antiferrodistortive distortion at the 22.6° STO GB21), giving rise to additional effects such as improper ferroelectricity43 and the rotostriction effect44 and thus influencing the electronic properties of the GB in a more complicated fashion.

Although GBs is well-known to play critical roles in the properties of oxide ceramics, the underlying mechanism is far from clear due to the intricacy. Among all the proposed mechanisms, elemental segregation-induced local nonstoichiometry45,46 is usually believed to be the dominant mechanism, which changes the local charge conditions and influences the transport properties47,48,49. In our study, the observed universal nanoscale flexoelectricity at GBs in these oxide ceramics provides a scenario to understand the electrical activities, i.e., the flexoelectric dipole carries “internal” polarization, and then, the bound charge must be screened by the “external” charges or it will not stably exist50, inducing charge (electron, oxygen vacancy, hole, etc.) redistribution and thus being expected to likewise influence the electrical activities. Furthermore, we built a structure that only has off-stoichiometry without huge strain gradients, showing a much smaller dipole moment (~9 μC cm−2) compared with the polarization of the trapezoidal cell in the GB core. Hence, the unique trapezoidal unit cell-induced flexoelectricity has a significant influence on the polar displacements and hence electrical activity. In this sense, the role played by the huge strain gradient-induced flexoelectricity is as important as the commonly believed elemental segregation for GBs.

In summary, we establish a systematic picture of nanoscale flexoelectricity at GBs, in which tunable and huge strain gradients can be achieved at the atomic scale. By the advanced STEM technique and theoretical DFT calculations, we determine the overall atomic structure of the exotic trapezoidal-like configuration in the GB, evaluate the strain gradients, quantify the atomic-scale flexoelectricity, reveal the electronic structure, and demonstrate the generality. Due to the huge strain gradients, large off-displacements of more than a hundred picometers can be achieved in the GB core with a polarized area typically within 3~4-unit cells. The presence of considerable flexoelectricity in the GBs and its universality provide insights into understanding the electrical activities of GBs in electroceramics.

Methods

Fabrication of bicrystals

A LAO bicrystal with a 24° mistilt GB was fabricated by using thermal diffusion bonding of two LAO single crystals at 1800 °C for 12 h in a N2 atmosphere under a uniaxial stress of 2 MPa. A STO bicrystal with a 36° mistilt GB was fabricated based on thermal diffusion bonding of two STO single crystals at 1000 °C for 10 h in a N2 atmosphere under a uniaxial stress of 2 MPa. The bicrystal was supplied by Hefei Ke Jing Materials Technology Co., LTD.

Preparation of TEM samples

The TEM specimens were first thinned by mechanical polishing and then subjected to argon ion milling. The ion milling process was carried out using a PIPS™ (Model 691, Gatan, Inc.) with an accelerating voltage of 3.5 kV until a hole was observed. Low voltage milling was performed with an accelerating voltage of 0.3 kV to remove the surface amorphous layer and minimize the irradiation-damaged layers.

Electron microscopy characterization and image analysis

HAADF and iDPC images were recorded at 300 kV using an aberration-corrected FEI Titan Themis G2. The convergence semiangle for imaging was 30 mrad, and the collection semiangle snap range was 4–21 mrad for iDPC imaging and 39–200 mrad for HAADF imaging. To obtain a sufficient signal-to-noise ratio for quantitative analysis, the iDPC image was acquired at 4096 × 4096 pixels, with a dwell time of 500 ms pixel−1 and a beam current of 20 pA to avoid beam damage.

To obtain quantitative information on the flexoelectricity, the atom positions were determined by simultaneous fitting with two-dimensional Gaussian peaks using a MATLAB code. The magnitude of the strain was defined as the difference in the lattice parameters between the strained and ground states. The strain was calculated based on the La (Sr) sublattice as \({{{{{{\mathrm{strain}}}}}}}=\frac{a\,-\,{a}_{0}}{{a}_{0}},\) where a0 is the lattice parameter of free-standing LAO (STO) and a is the in-plane lattice parameter perpendicular (az) or parallel (ax) to the GB plane. The strain gradient was then obtained by taking the differential of the strains along different directions, given as d(ezz)/dz = 2 * (\({e}_{{zz}}^{n}\) − \({e}_{{zz}}^{n-1}\))/(\({a}_{z}^{n}\) + \({a}_{z}^{n-1}\)) and d(ezz)/dx = (\({e}_{{zz}}^{m}\) − \({e}_{{zz}}^{m-1}\))/\({a}_{x}^{m}\)). In Fig. 1b, we recognize side c as the lattice parameter (a0) of the free-standing state. GPA was performed using the free FRWRtools plugin for Digital Micrograph (developed by Kotch et al. and available at https://www.physics.hu-berlin.de/en/sem) based on the original work31.

A previous study51 suggested that the error in displacement measurement mainly comes from misalignments (e.g., specimen mistilt and residual lens aberration). In our work, we conducted careful alignment to minimize the artifacts. We set the center of the Ronchigram of the GB to the alignment center when acquiring the image, as shown in Supplementary Fig. 2a. The corresponding Ronchigrams of two surrounding grains are also shown in Supplementary Fig. 2b, c. Then, the offset between the center of the Ronchigram of surrounding grains and the alignment center indicates the deviation from their on-zone axis orientations (nearly 1.7 mrad, corresponding to 0.1°). Based on the experimental parameters, we performed a QSTEM software simulation (https://www.physics.hu-berlin.de/en/sem/software/software_qstem). The results show that such crystal tilts will result in ~1 pm false displacement measurements (Supplementary Fig. 2d). Furthermore, the surrounding grains away from the GB core were regarded as the reference polarization-free structure and analyzed to evaluate the mistilt effect. Then, the displacements in the reference LAO and STO were measured as 4.3 ± 1.8 pm (Supplementary Fig. 2e) and 4.8 ± 1.6 pm, showing good agreement with the previous iDPC image error level (typically ~5 pm51). The discrepancy between the simulation and experiment mainly arises because the experimental error comes from not only mistilt noise but also scanning noise and specimen drift in acquiring STEM images30. Nevertheless, the error level is typically one order below our flexoelectric displacement (~81.4 pm), proving the data reliability. To further minimize the fluctuation between different locations, the estimated displacements in the GB core were averaged among the periodic structural units to present the key features.

Four-dimensional scanning electron diffraction (4D-STEM) characterizations

Scanning diffraction data sets were collected by using a Nion HERMES 200 microscope operated at 60 kV. The probe convergence semiangle was 35 mrad. The sample thickness was estimated as ~6 nm. All acquired 4D data sets were processed by custom-written Python code based on the GetDPC package52. However, such phase contrast in 4D-STEM mode is very sensitive to the crystal tilt53 and thickness variation and limit54. Thus, achieving an accurate conclusion regarding the quantitative charge analysis for GBs from 4D-STEM measurements remains challenging due to the presence of small misalignment between two grains, stress relaxation in the ultrathin specimen, and possible thickness differences across the GB.

EELS characterizations and analysis

STEM-EELS spectra were recorded using a Nion HERMES 200 microscope. To reduce beam damage, EELS experiments were performed at 60 kV. The probe convergence semiangle was 35 mrad, and the collection semiangle was in the range of 24.9 mrad. We acquired a single 25 × 70 pixel EELS map from a 4.27 × 16 nm region containing the GB. The dwell time was 150 ms pixel−1, and the dispersion was 0.1663 eV ch−1. The data were smoothed by a Gaussian-weighted moving average filter with a window length of 7 channels and a variance of 1 channel. The extracted EELS spectra in Fig. 4b, d were spatially averaged over the regions parallel to the GB plane (marked by the rectangle in Supplementary Fig. 6b). The EELS background was fitted and subtracted using the power law \(I\left(\triangle E\right)={A}_{0}\cdot {\triangle E}^{-r}\). The L3/L2 ratio calculation was based on the spectral integral intensity ratio of the 77.2–78.8 eV and 79.3–80.9 eV energy windows. The fitting uncertainty was estimated by the standard deviation among rows.

First-principles calculations

Electronic structure calculations were performed using the Vienna Ab initio Simulation Package (VASP)55,56. The projected augmented wave (PAW)57,58 potential was used to address with the interactions between ions and electrons. The exchange-correlation potential was treated by the Perdew–Burke–Ernzerhof59 functional. A plane-wave cutoff of 600 eV was used. For the bulk rhombohedral structure, the experimental lattice constants (a = b = c = 5.360 Å, α = β = γ = 60.011°) were used. Then, the bulk pseudocubic structure was used as a block unit to build the GB structure60. Atomic positions were relaxed until the maximum force was less than 0.01 eV Å−1. Band structures were obtained at the DFT level. For the GB, we found that the charge-neutral system is gapless. Thus, to make the system have a finite gap, extra four electrons were added to the cell. Born effective charges were computed using density functional perturbation theory61,62,63.

The polarization calculation was based on the equation of spontaneous polarization Ps = \(\frac{1}{V}\sum {\delta }_{i}{Z}_{i}\)64, where \({V}\) is the volume of the unit cell, \(\delta\) is the displacement of atom, \(i\) from its centrosymmetric position and \(Z\) is the Born effective charge of atom \(i\). \(\delta\) was evaluated from the displacements of each column with respect to the corresponding position in the polarization-free bulk crystal. The charge density was calculated within the DFT in the VASP package.