Construction Materials and Technologies June 28 June 30, 2010, Universit Politecnica delle Marche, Ancona, Italy. Main Proceedings ed. J Zachar, P Claisse, T R Naik, E Ganjian. ISBN 978 1 4507 1490 7 http://www.claisse.info/Proceedings.htm
ABSTRACT
The development of alkali activated binders with superior engineering properties and longer durability has emerged as an alternative to OPC. It is possible to use alkali-activated natural pozzolans to prepare environmentally friendly geopolymeric cementitious construction materials. The main benefit of geopolymers cements is their reduction in environmental impact leading to the concept of sustainable development. This paper presents a summary of and experimental study on the engineering properties of geopolymer concrete prepared with Taftan andesite, an activated Iranian natural pozzolan. Experimental work was conducted to determine mechanical strength; modulus of elasticity; ultrasonic pulse velocity of different concrete mixtures. Test data have been used to identify the effects of salient factors such as water to binder ratios and curing conditions that influence the properties of the geopolymer concrete. The results show that mortar and concrete made with the alkali activated natural pozzolan develop moderate to high mechanical strength and modulus of elasticity.
INTRODUCTION
Concrete made with Portland cement is a major construction material used worldwide. Unfortunately, the production of Portland cement releases large amounts of CO2 into the atmosphere making a major contribution to the greenhouse effect and the global warming of the planet. Portland cement production is estimated to contribute around 7% of global CO2 emissions. To reduce greenhouse gas emissions, efforts are needed to develop environmentally friendly construction materials. One such alternative is geopolymer cement which can be utilized to manufacture pre-cast concrete, structural and non-structural elements, immobilize toxic waste, and produce concrete products that are resistant to heat and aggressive environments [Hardjito et al., 2004a, 2004b]. Unlike regular concrete, the chemical reactions that form the geopolymer concrete alternative do not require high temperatures for processing which give off carbon dioxide. The geopolymer concrete
manufacture is estimated to reduce CO2 emission by 22% to 72% (depending on materials used) compared to OPC production [Bondar, 2009]. This paper presents the technology of making geopolymer concrete using a natural pozzolan as its source material and presents the results of laboratory tests conducted on this material. The research data presented in this paper are useful to understand the engineering properties of geopolymer concrete.
yield different reaction products without detracting from material durability, because according to Fernandez, Palomo, and Hombradoz (2006), increases in the curing temperature go hand-in-hand with decreases in the amount of Al incorporated into the final product and a concomitant improvement in mechanical properties. Such improvements parallel the formation of a homogeneous aluminosilicate matrix [Davidovits, 1999]. Puertas et al. (2003) reported that the elastic modulus of OPC mortars was 5.7 GPa, higher than the values for PFA mortars activated with 8M NaOH (4.4 GPa). Fernandez-Jimenez et al. (2006) found that the addition of soluble silicates in the alkaline solution improved the modulus of elasticity in PFA-based geopolymer concrete. However, this improvement was not sufficient and the alkali activated PFA concrete showed a much lower static modulus of elasticity than expected. The values presented for OPC concrete ranged from 30.3 to 32.3GPa while for geopolymeric concrete they ranged from 10.7 (without silicate) to 18.4 GPa (with silicate). Hardjito et al. (2004) observed better elastic modulus results for fly ash based geopolymer concrete samples: 22.95 to 30.84 GPa.
Table 1 Physical and chemical composition (oxide percent) of the materials used in this investigation
Surface Material LOI SiO2 Al2O3 Fe2O3 CaO MgO TiO2 K2O Na2O area (cm /g) Taftan andesite 1.85 61.67 15.90 4.32 7.99 2.04 0.438 2.12 3.21 3836 2.22
2
SG
Potassium hydroxide (KOH) pellets supplied by MERK International Ltd. were dissolved in water to produce the alkaline solutions for geopolymer concrete production. Sodium silicate solution was provided by Iran Silicate Industrial Company in the form of water glass. The chemical composition of the solution provided by the manufacture was: 8.5% of sodium oxide (Na2O), 26.5% of silicon oxide (SiO2) and 65% of water; pH=11.4. The aggregate used in this study was obtained from the Karaj River deposits in the northwest of Iran and comprised 14mm and 4.75mm coarse aggregates and fine sand. The fineness modulus of the combined aggregates was 2.08. The proportioning of the control concrete mixture was based on the BRE method [Neville, 1995] targeting a 40 MPa (28 days) compressive strength and a slump of 60 mm. The cement
was substituted with the same quantity of natural pozzolan plus the solids in water glass and alkaline solution but no additional water was added as the activators were already in solution. The amount of solids in water glass and alkaline solution to total binder ratio by mass was 20 and 25% for ATAF1 and ATAF2 mixes, respectively and the ratio of KOH (ml)/ Na2SiO3 (ml) was 7.7 for all mixes. The notation for the mixes is as follows: CM1: PC control mix with w/c=0.45 CM2: PC control mix with w/c=0.55 ATAF1: Activated Taftan pozzolan with w/b=0.45 ATAF2: Activated Taftan pozzolan with w/b=0.55 Activated Taftan pozzolan mixes with w/b of 0.4 and 0.5 were also tested for the measurement of compressive strength.The concrete samples were cast in different sizes as required by the tests. The mixtures were cast into the pre-oiled moulds in three layers and vibrated by means of a vibrating table to remove any entrapped air. The flow of the mixtures was measured by vebe test and the vebe times were 25 and 12 seconds for ATAF1 and ATAF2 mixes, respectively. It was observed that a geopolymer concrete stick hard to the mould and oiling of the moulds is very important to release the samples. Taftan specimens were de-moulded 24 hours after casting and cured in two curing regimes and at three different temperatures: 1) Sealed curing: Three series of specimens were sealed wrapped in a special plastic covering which was tested to be impermeable and stored in a controlled room kept at 202, 402 and 602C. 2) Fog curing: Three series of the specimens were cured in the fog chamber set at three different temperatures equal to 202, 402 and 602C for the measurement of compressive and splitting tensile strength. Fog curing at 402C was used for static modulus of elasticity test.
Testing Procedures
In order to determine the compressive strength of geopolymer concrete each mixture was prepared as 100x100x100 mm cubes and the compressive strength for these samples were tested according to BS EN 12390-3:2009. Details of casting and curing are described in section 3.1. Three samples of each formulation were tested at 1, 7, 14, 28, 90, 180 and 365 days, and the average compressive strength values reported as the results. The ultrasonic pulse velocity was measured in accordance with BS EN 12504-4-2004. The measurement was conducted on the 100mmx100mm end face of a prism with a length of 500mm. Duplicate sets of samples were tested at 28, 90,180 days. The splitting tensile strength of all mixes was measured using 100mm x 200mm length cylinders. The samples were prepared and splitting tensile tests performed as described in BS EN 12390-6:2002. The specimens were tested in duplicate sets at 7, 14, 28, 90, 180 days and the average results are reported. The static modulus of elasticity was determined according to BS1881-121:1983 standard by subjecting a 100mm x 200mm cylinder specimen to uni-axial compression and measuring the deformation by means of dial gauges fixed between certain gauge lengths. Dial gauge reading divided by gauge length gives the strain while load applied divided by area of cross section gives the stress. A series of readings were taken and the stress-strain relationship
established. The modulus of elasticity found from actual loading is called static modulus of elasticity.
50
50 40 30 20 10 0 1
Compressive Strength(MPa)
45 40 35 30 25 20 15 10 5 0 1 Age(days)10
20Sealed 20Fog 40Sealed 40Fog 60Sealed 60Fog OPC-20Sealed 100 1000 OPC-20Fog
35 30 25 20 15 10 5 0 1 10 Age(days)100
20Sealed 20Fog 40Sealed 40Fog 60Sealed 60Fog 100 1000 OPC-20Sealed OPC-20Fog
Fig. 1 Effect of different curing condition and curing temperature oncompressive strength development for activated Taftan pozzolan with different water to binder ratios (the fluctuations in strength results are probably due to sample to sample variability)
The effect of water content is illustrated in Figure 2 by plotting the 28 days compressive strength versus water-to-geopolymer solids ratio by mass. The test data shown in Figure 2 demonstrate that the compressive strength of geopolymer concrete decreased as the ratio of water-to geopolymer solids by mass increased giving rise to more free water in the geopolymer concrete leading to a more porous microstructure. The trends of these test results are similar to those observed by Hardjito et al (2004c) and Barbosa et al (2000) for their tests on geopolymer concretes. The results shown in Figure 2 also confirm that an increase in the curing temperature increased the concrete compressive strength.
55
20Sealed 45 35 25 15 5 0.35 0.4 0.45 0.5 0.55 0.6 20Fog 40Sealed 40Fog 60Sealed 60Fog
Fig. 2 Compressive strength at 28 days versus water to binder ratio (W/B) for alkali activated Taftan pozzolan at different curing temperature Ultrasonic Pulse Velocity
Figure 3 shows the results for the ultrasonic pulse velocity test for all mixes. ATAF1 achieved the highest values followed by ATAF2 which has a higher w/b. All of the geopolymer concrete mixes showed lower ultrasonic pulse velocities than the OPC concrete mixes, even with the same or higher compressive strength.
5.5 5
UPV(km/sec)
4.5 4
Fig. 3 Ultrasonic Pulse Velocity for different mixes Indirect Tensile Strength
The results of the indirect tensile strength tests up to 180 days are shown in Figure 4. The trend in tensile strength is similar to that obtained for compressive strength. Figure 4 illustrates there was a difference in the development in tensile strength of different mixes. As far as the geopolymer concrete mixes based on activated natural pozzolan are concerned, higher strengths were observed at longer ages in comparison with control OPC mixes. At early age, ATAF2 showed lower tensile strength results than the OPC control mix, 1.7MPa compared to 2.03MPa while the ATAF1 mix gave 3.57 MPa after 28 days, higher than the corresponding OPC control mix at 2.67Mpa. The results show that the long term tensile strengths of activated Taftan geopolymer concrete mixes are higher than those of OPC control mixes, 3.69 and 3.0 MPa after 365 days compared to CM1 and CM2 at 2.81 and 1.99, respectively. The tensile strength of activated natural pozzolan geopolymer concrete is more sensitive to improper curing than its compressive strength, the same as in OPC concrete. Figure 4 illustrates the effect of curing conditions and temperatures on tensile strength of concrete made from activated natural pozzlans. The optimum temperature of curing was 40C, the same as that found for compressive strength. Figure 4 also shows that a higher water to binder ratio resulted in lower tensile strength, the same trend as for OPC mixes.
Age (days)
100
Fig. 4 Effect of different curing conditions and curing temperature on Indirect Tensile strength development for ATAF1 and ATAF2 mixes Static Modulus of Elasticity
Results of the static modulus of elasticity are shown in Figure 5. In a similar way to the compressive strength results, the static modulus of elasticity increased with age. This improvement was rapid in the first 28 days as most of the modulus value was generally achieved in this period. During the first 14 days the mixes made with activated natural pozzolans have mostly shown lower values of static modulus of elasticity than OPC concrete mixes, except for the ATAF1 mix. The static modulus of elasticity for ATAF1, ATAF2 mixes after 14 days was 33.96, 14.03GPa at 40C curing temperature, respectively with that for the CM1 mix was 26.55GPa. Long term results show that the static elastic modulus of some of alkali activated natural pozzolans such as ATAF1 are around 5% to 20% more than OPC mixes. The long term static modulus of elasticity of ATAF1, ATAF2 mixes were 32.7, 26.8GPa compared to OPC concrete mixes which gave 29GPa. The elastic modulus was affected by the curing temperature. At early ages the static modulus of elasticity increased with increasing the curing temperature up to a limit which seems to be related to the water to binder ratio (Figure 5). For ATAF1 with a water to binder ratio of 0.45, the elastic modulus increased with increasing curing temperature up to 40C but decreased when the curing temperature rose to 60C. For ATAF2 mixes where the water to binder ratio was 0.55, the temperature where the highest static modulus of elasticity was obtained rose to 60C. However, over the long term the results drop to the same value as the mix cured at 40C.
35 30
(GPa)
30 25
(GPa)
25 20 15 10 5 0 0 50 (days) 100 Age 20Sealed 40Sealed 40Fog 60Sealed CM1-20Sealed 150 200
20 15 10 5 0 0 50 100 Age (days) 20Sealed 40Sealed 40Fog 60Sealed CM2-20Sealed 150 200
Fig. 5 Effect of different curing condition and curing temperature on Static Modulus of Elasticity development for ATAF1 and ATAF2 mixes CONCLUSIONS
The main conclusions drawn from this investigation of the engineering properties of geopolymer concrete made from activating natural pozzolans (i.e. alkali activated natural pozzolan or AANP) are summarized as follows: 1) Geopolymer concrete from activated natural pozzolans generally shows lower strengths than OPC mixes at early ages, but they reach the same or even higher strengths than OPC mixes after long-term curing. 2) The strength of geopolymer concrete decreases as the ratio of water to geopolymer solids by mass increases. This allows more entrapment of water within the geopolymer paste and makes a looser microstructure in this type of concrete. 3) It seems that the ultrasonic pulse velocity in the geopolymer concrete is lower than in OPC concrete of the same compressive strength. 4) During the first 14 days, activated natural pozzolan concrete mixes generally have lower values of static modulus of elasticity than OPC concrete mixes. However, the long term results show that the static elastic modulus of alkali activated natural pozzolans concrete is generally around 5 to 20% higher than for OPC mixes. 5) The elastic modulus of AANP concrete is affected by the curing temperatures. At early ages the static modulus of elasticity increased with increasing curing temperature to a limit which seems to be related to the water to binder ratio. If water is lost due to evaporation when curing at higher temperature before the full strength is gained, the static modulus of elasticity decreases.
REFERENCES
Barbosa, V.F.F., K.J.D. MacKenzie, and C. Thaumaturgo (2000), Synthesis and characterisation of materials based on inorganic polymers of alumina and silica: sodium polysialate polymers, International Journal of Inorganic Materials, Vol. 2, pp. 309-317 Bondar, D. (2009), "Alkali Activation of Iranian Natural Pozzolans for Producing Geopolymer Cement and Concrete", A dissertation submitted to University of Sheffield in fulfilment of the requirements for the degree of Doctor of Philosophy, U.K Davidovits, J. (1999), Chemistry of Geopolymeric Systems, Terminology, Presented at the Geopolymer 99 International Conference, France Ezatian, F. (2002), " Atlas of Igneous Rocks: Classification and Nomenclatures", Ministry of Industries and Mines, Geological Survey of Iran (GSI) (in Farsi) Fernandez-Jimenez, A. M., A. Palomo, et al. (2006), "Engineering properties of alkali activated fly ash concrete." ACI - Materials Journals 103(2), pp. 106-112 Hardjito, D., S.E. Wallah, D.M. J. Sumajouw, and B.V. Rangan (2004a), On The Development of Fly Ash-Based Geopolymer Concrete, ACI Materials Journal, Accepted for publication Hardjito, D., S.E. Wallah, D.M. J. Sumajouw & B.V. Rangan (2004b), The StressStrain Behaviour of Fly Ash-Based Geopolymer Concrete, in ACMSM 18,A.A. Balkema Publishers - The Netherlands, Perth, Australia Hardjito, D., S.E. Wallah, D.M. J. Sumajouw & B.V. Rangan (2004c), "Factors influencing the compressive strength fly-ash based geopolymer concrete", Jurusan Teknik Sipil, Fakultas Teknik Sipil dan Perencanaan Universitas Kristen Petra, Vol. 6, No. 2, pp.88-96 Neville, A. M., (1995), "Properties of Concrete", Essex, England, Pearson Educational Limited Palomo, A., M.T. Blanco-Varela, M.L. Granizo, F. Puertas, T. Vazquez, and M.W. Grutzeck (1999a), Chemical stability of cementitious materials based on metakaolin, Cement and Concrete Research, Vol. 29, pp. 997-1004 Palomo, A., M.W. Grutzeck, and M.T. Blanco (1999b), Alkali-activated fly ashes, a cement for the future, Cement and Concrete Research, Vol. 29, pp. 1323-1329 Puertas, F., Amat, T., Fernandez-Jimenez, A., Vazquez, T. (2003), Mechanical and durable behaviour of alkaline cement mortars reinforced with polypropylene fibres, Cement and Concrete Research, 33, pp.20312036 Rowles, M. and B. OConnor (2003), Chemical optimisation of the compressive strength of aluminosilicate geopolymers synthesised by sodium silicate activation of metakaolinite, Journal of Materials Chemistry, Vol. 13, pp. 1161-1165 Van Jaarsveld, J.G.S., J.S.J. Van Deventer, and G.C. Lukey (2002), The effect of composition and temperature on the Properties of fly Ash and kaolinite-based geopolymers, Chemical Engineering Journal, Vol. 89, pp. 63-73 Van Jaarsveld, J.G.S., J.S.J. Van Deventer, L. Lorenzen (1997), The potential use of geopolymeric materials to immobilise toxic metals: Part I. Theory and applications. Miner, Eng. 10 _7, pp.659669 Xu, H., J.S.J. Van Deventer (2000), The geopolymerisation of aluminosilicate minerals, International Journal of Mineral Processing, Vol. 59, pp. 247-266