17th World Conference on Nondestructive Testing, 25-28 Oct 2008, Shanghai, China

The difference among three reference standards used in the


performance evaluation of wire rope EMT instrument
Hougui CHEN 1, Yihua KANG 2, Jiangjun RUAN 1
1

School of Electrical Engineering, Wuhan University; Wuhan, China

Phone: +86 027 68775439; E-mail: hougui_ch@163.com, ruan308@126.com


2

School of Mechanic Engineering, Huazhong University of Science and technology; Wuhan, China
Phone: +86 027 87556941; E-mail: yhkang@263.net

Abstract
A reference standard for a unit of measurement is an artifact that embodies the quantity of
interest in a way that ties its value to the reference base. The selection of an appropriate reference
standard is a crucial point in the performance evaluation of wire rope electromagnetic testing
(EMT) instrument. In this paper, a 3-D finite element model (FEM) has been developed to study
three reference standards. The effects of the magnetizing ampere-turn, the loss of metallic
cross-sectional area on the main magnetic flux and the structure have been addressed. Comparison
analyses have been made of the simulation results of the three reference standards.
Keywords: Finite element method; Nondestructive testing; Reference standard

1. Introduce
Wire rope EMT instrument is an important instrument used in wire rope safety inspection,
and its testing precision effects on the result of wire rope condition evaluation significantly. In
ASTM E 1571, a summary contend is presented to rule the wire rope EMT instrument, in the item
10.3, the rod bundle reference standard is introduced to evaluate the performance on measuring
the loss of metallic cross-sectional area [1]. In practice, a standard composed of a pipe and a bundle
of rods is used; however, the wire rope is a special component with complex helix structure, and
there are great differences between the reference standard and the wire rope; therefore, pipe
standard is just a cursory substitute, and may cause evaluation error. It is significant to reveal the
difference between the wire rope and its substitutes so as to choose reference standard in reason.
Large amount of references focus on the pipe EMT and wire rope EMT [2-5], but few papers are
found to concentrate on the difference of magnetic performance between the wire rope and it
reference standards.
In this paper, three standards have been chosen to research on their difference in magnetic
character. The FEM, the most effective method to study on EMT question related to more
important detail inner material, was applied to bring enough data.
Our research aims at selecting an appropriate reference standard for Wire rope EMT
instrument. The approach is to investigate the magnetic character difference of three reference
standards: a pipe with rod bundle, a strand and a pipe. Utilizing finite element model (FEM),
numerical simulations have been conducted to investigate the difference among three reference

standards studies are also conducted to investigate the effects of the magnetizing ampere-turn and
the loss of metallic cross-sectional area on the main magnetic flux. Comparison analyses have
been made of the simulation results.

2. The principle of EMT on the loss of metallic cross-sectional area


The test principle of the loss of metallic cross-sectional area of wire rope electromagnetic is
shown in Fig.1. The exciter coil produces enough magnetizing energy to magnetize the wire rope,

Fig. 1 Principle of wire rope EMT

then, the main magnetic flux, which passes through the cross section of wire rope, will be changed
significantly when flaw lies in the wire rope, the measuring coil detect this change, finally, the
change is converted into a reason result of the loss of cross-sectional area.
The EMT can be simplified as a magnetic resistant model as shown in Fig.2, where Rs is the

Fig. 2 Equivalent magnetic circuit of EMT of wire rope

magnetic resistant of wire rope, Ra1 and Ra2 is the magnetic resistant of air between the yoke and
the wire rope, Ry1 and Ry2 is the magnetic resistant of the yoke, Rc is the inner magnetic resistant
of the exciter coil, F is the magneto-motive forces of EMT system. F can be expressed as:

F = ( R y1 + R y 2 + Ra1 + Ra 2 + Rc + Rs )

(1)

where is the magnetic flux through the main magnetic circuit.


Equation (1) leads to:

F
Ry1 + Ry 2 + Ra1 + Ra 2 + Rc + Rs

(2)

Equation (2) shows thatis determined by Ry1, Ry2, Ra1, Ra2, Rc and Rs, and it has a linear
relationship with Rs when Ry1, Ry2, Ra1, Ra2 and Rc are regarded as immobility parameter
According to Fundamental theory of Circuit, the magnetic resistance is inversely proportional to
2

the cross-sectional areas. Therefore, there is a linear relationship between the main magnetic flux
and the cross-sectional area of wire rope. In really world, the parameters above are variable and
the geometries of the cross-section of wire rope have significant effects on the main magnetic flux
and the performance evaluation of EMT instrument.

3. Calculation and analysis


In order to analysis the magnetic difference among the three reference standards, a 3-D FEM
has been developed as shown in Fig.3. The scale of figure adjusted to make the structure more
clear. Exciter coil was adopted to provide enough magnetic energy to magnetize the reference

Fig. 3. Finite element model of EMT of standard

standards. In order to enhance magnetizing efficiency, a pair of cylinder yokes was set between the
exciter coil and the reference standard, the reference standard was placed inner the yoke. The air
gap between the yoke and the surface of reference standard is 1mm; the length of exciter coil is
140 mm.
The element type used in this model is solid117. Sweep mode and intelligent mode are used
to mesh the model according to the difference of components; a typical 3-D meshing in Fig. 4. The
material of standards is nonlinear, their B-H curve is shown in Fig. 5, the material of yoke is linear,
and its relative magnetic permeability of material is 1000. The relative magnetic permeability of
exciter coil material is 1. The relative magnetic permeability of other air space is 1. During the

Fig. 4. Model meshing

Fig. 5. B-H curve of standard

course of EMT analysis, designed ampere-turn current was imposed on the exciter coil; then,

results were obtained through a designed program; the axis component of magnetic strength are
mapped onto a series of path. The middle cross-section (shows in fig. 1 in o-o) was partitioned
into 28800 subfields, the magnetic strength of every subfield are abstracted to form the magnetic
condition of middle cross section. At last, the total magnetic flux of o-o was calculated by
MATLAB program and subsequently data analysis is also done using MATLAB program.

3.1 Difference when imposing the same series of ampere-turns.


Three standards are chosen to analysis the difference between wire rope and its substitutes.
The strand is similar with the wire rope in structure, therefore can present some common character
of helix structure; furthermore, analysis with strand can reduce calculation because wire rope can
result in large amount of calculation that can be beyond the competence of ANSYS. The reason
why Pipe is chosen is that solid structure may be much closer to the wire rope therefore may be
much fitter as a substitute. Figure 6 is the cross section of three reference standards, for the first
reference standard, the outer diameter of pipe is 15 mm, the thickness of pipe is 3.35 mm, the

Fig. 6. Cross section of standards

diameter of rod is 1.34 mm, and the number of rods is 12, and the cross-sectional area of rod is
close to 1% of total cross-sectional area of standard. For the second standard, the diameter of pipe
is 15 mm, and its thickness is 4.1 mm. For the third standard, the outer diameter of strand is 15
mm, the diameter of wire is 5 mm, and the number of wire is 7. The area of three standards shows
in table 1.
Table 1:
Diameter

Cross-sectional area

error

Pipe with rods

15

140.4

0.2%

Strand

15

140.1

0%

Pipe

15

139.5

0.4%

200, 400, 800, 1000, 2000, 3000, 4000, 6000, 8000 and 10000 ampere-turn are imposed on
the three simulation models in sequence. Curves between the main magnetic flux and the
ampere-turn show in figure 7. Figure 7 shows that the curves are similar with the B-H curve of

Fig. 7. Relationship between the main magnetic flux

Fig. 8. Magnetic strength in the pipe wall

and the ampere-turn EMT of wire rope

steel material shows in fig. 5. The main magnetic flux of pipe is larger than that of strand, and the
main magnetic flux of strand is larger than that of pipe with rods. The reason that results in this
phenomenon is that the magnetic field in the research area is not so uniform; figure 8 is the curve
between the axis component of magnetic strength and the position along the outer surface to the
inner surface of the pipe. Figure 8 shows that there are a start area, a steady area and an end area,
in the start area, the magnetic field increase from a low level to a high level; in the steady area, the
magnetic field is uniform; in the end area, the magnetic field decrease from a high level to a low
level. This phenomena lie in every single body, so different distribution of metal can result from
different total main magnetic flux; therefore, the metal is more compacter, the main magnetic flux
is larger.
3.2. Difference when making the same loss of metallic cross-sectional area
Calculation is carried out to analysis the sensitivity difference of the three standards on the
loss of metallic cross-sectional area. Two methods are applied to create the loss of cross-sectional
area; for the pipe and the strand, the method is cutting out some surface metal in sequence to
simulate the wear; for the pipe with rods bundle, the method is moving out some rods in sequence
to simulate the vary of cross-sectional area. The ampere-turn imposed on the model is 6000, the
loss used to analysis the difference in sensibility in loss of metallic cross-sectional area is 0%, 2%,
4%, 6%, 8%, 10%, 12%. Figure 9 shows the sequence of loss of cross-sectional area, the area

Fig. 9. Simulation of loss of metallic cross-sectional area of standards

error rate of every change is under 0.1%. Curves between the main magnetic flux and the loss of
metallic cross-sectional area show in figure 10. Figure 10 shows that the main magnetic flux is
well linear with the loss of cross-sectional area that means that three standards have similar

Fig. 10. Curves between the main magnetic flux and the rate of loss of cross-sectional area

sensitivity to the loss of metallic cross-sectional area; therefore, an instrument can make similar
evaluating result by different standard. But the working point of three standard are dissimilar, the
highest is the pipe, and then is the strand; the lowest is the pipe with rods bundle.

4. Discussion and conclusion


Wire rope is a special component, a common wire rope is compose of 3 mainly units, the core,
the king wire and the strand. In order to produce a wire rope, firstly Wire screw around the king
wire and make a strand, during this period, the wire is 1 time helix cylinder; secondly, strands
screw around the core and make a rope, during this period, the wire is 2 time helix cylinder.
Therefore, the wires are inter twisted together, and it is very difficult to make exact loss of
cross-section, and the substitute must be use when evaluating a wire rope EMT instrument.
ASTM E 1571 calls for rod bundle reference standard as a substitute of wire rope to evaluate
the inspecting performance on loss of metallic cross-sectional area. In practice, a pipe with rod
bundle in it may be more convenient because it can uniform the outer diameter of reference
standard and avoid some influence result from the position change of rods.
It is very difficult for EMT instrument custom to keep uniform distribution of rod; therefore,
different evaluation results can be made by different evaluators. Pipe reference standard is prone
to uniform; the wear is easier to make using standardization procedure.
Data shows that pipe standard and pipe standard with rod bundle are similar with strand
standard which is a representation of wire rope in magnetic performance. When imposing current
density on the standards in sequence, the curve of main magnetic flux are similar, but the working
points are dissimilar, the highest is the pipe, and the follower is the strand, and the lowest is the
pipe with rod bundle in it. When change the cross-sectional area of standard in sequence, the main
magnetic flux of three standards are similar in sensitivity in the loss of metallic cross-sectional
area, but the working points are dissimilar, the highest is the pipe, and the follower is the strand,
and the lowest is the pipe with rod bundle in it.

Reference
1.

ASTM E1571-01 Practice for electromagnetic examination of ferromagnetic steel wire rope.
6

2.
3.
4.
5.

ASTM standard, November, 2001.


Geller, L. B., Leung, K. J., Udd, E., et al. Electromagnetic Testing of Wire Ropes-New
Developments. CIM Bulletin, Oct 2003, 96(1074): 65~71
Chaplin, C. R., Ridge, I. M. L.. Measurement of Abrasive Wear on Wire Ropes Using
Non-destructive Electro-magnetic Inspection. OIPEEC Bulletin, 78(1999): 67~80
Yong Li, Gui Yun Tian. Numerical simulation on magnetic flux leakage evaluation at high
speed. NDT&E Int., 2006, v39(5): 367-373
Mao W. etc.. Effects of alignment of nearby corrosion pits on MFL. NDT&E Int., 2003,
v36(2): 111-116