Acidur 4404

TECHNICAL DATA SHEET


X2CrNiMo17-12-2
1.4404

AUSTENITIC STAINLESS STEEL

CHEMICAL COMPOSITION (IN WEIGHT-% ACCORDING TO DIN EN 10088-3)

C Si Mn P S Cr Mo Ni N

min. - - - - - 16.5 2.0 10.0 -

max. 0.03 1.0 2.0 0.045 0.03 18.5 2.5 13.0 0.1

CHEMICAL COMPOSITION (IN WEIGHT-% ACCORDING TO ASTM A276)

C Si Mn P S Cr Mo Ni N

min. - - - - - 16.0 2.0 10.0 -

max. 0.03 0.75 2.0 0.045 0.03 18.0 3.0 14.0 0.1

Customer specific limitations of standard analysis are possible after consultation with the Deutsche Edelstahlwerke GmbH.

APPLICATIONS
GENERAL PROPERTIES
Acidur 4404 is one of the common corrosion- Corrosion resistance very good
resistant stainless steels. Due to its molybdenum Mechanical properties average
content, it offers a high degree of resistance against Forgeability good
non-oxidising acids and halogenated media. Further- Weldabilty excellent
more, Acidur 4044 is easy to process and can be used Machinability average
at temperatures up to 550°C.

SPECIAL PROPERTIES

STANDARDS AND DESIGNATIONS » Polishable


DIN EN 10088-3 1.4404
» Resistant to intergranular corrosion
X2CrNiMo17-12-2
in continuous operation up to 300°C
AISI 316L
» Suitable for low temperatures
» Suitable for use at temperatures
03/06/2016 2016-0036 Page 01

UNS S31603
JIS SUS316L
up to 550°C
B.S. 316S11
SS 2348
AFNOR Z3CND17-11-02
Acidur 4404
TECHNICAL DATA SHEET
X2CrNiMo17-12-2
1.4404

PHYSICAL PROPERTIES TYPICAL APPLICATIONS


Density in kg/dm3 8.0 » Chemical and pharmaceutical industry
Electrical resistivity 0.75 » Food industry
at 20°C in (Ω mm2)/m » Fittings and plant engineering
Magnetisability low1 » Construction industry
Thermal conductivity 15 » Offshore
at 20°C in W/(m K) » Petrochemistry
Specific heat capacity 500 » Automotive industry
at 20°C in J/(kg K) » Decorative items and kitchen utensils
Young's modulus in GPa at » Electronical equipment
» 20°C 200 » Aerospace
» 100°C 194 » Mechanical engineering
» 200°C 186
» 300°C 179 Note: Delivery according to building approval Z-30.3-6
and pressure vessel standard DIN EN 10272.
» 400°C 172
» 500°C 165
Thermal expansion coefficient
in 10-6K-1
PROCESSING PROPERTIES
» 20°C - 100°C 16.0 Machining yes
» 20°C - 200°C 16.5 Hammer and die forging yes
» 20°C - 300°C 17.0 Cold forming yes
» 20°C - 400°C 17.5 Cold heading yes
» 20°C - 500°C 18.0 Polishability yes

1
The material can be magnetised in quenched TEMPERATURES FOR HOT FORMING
condition. With increasing cold forming the magnetisability
increases, too.
AND HEAT TREATMENT

HOT FORMING
Temperature in °C Cooling1
1200 - 900 air, water
03/06/2016 2016-0036 Page 02

HEAT TREATMENT
Temperature in °C Cooling1
Solution annealing (+AT) 1020 - 1120 water, air

depending on dimension
1
Acidur 4404
TECHNICAL DATA SHEET
X2CrNiMo17-12-2
1.4404

MECHANICAL PROPERTIES IN SOLUTION ANNEALED CONDITION (+AT)


AT ROOM TEMPERATURE ACCORDING TO DIN EN 10088-3

Ø in mm Hardness Rp0.2 in MPa Rp1.0 in MPa Rm in MPa A5 in % AV in J Z in %


in HB

longitudinal transverse longitudinal transverse

≤ 160 ≤ 215 ≥ 200 ≥ 235 500 - 700 ≥ 40 - ≥ 100 - -

160 < d ≤ 250 ≤ 215 ≥ 200 ≥ 235 500 - 700 - ≥ 30 - ≥ 60 -

For thicker dimensions (d > 250 mm) the mechanical properties have to be agreed.

MECHANICAL PROPERTIES IN SOLUTION ANNEALED CONDITION (+AT)


AT ROOM TEMPERATURE ACCORDING TO ASTM A276

Ø in mm Hardness Rp0.2 in MPa Rp1.0 in MPa Rm in MPa A2'' in % AV in J Z in %


in HB

longitudinal transverse longitudinal transverse

all - ≥ 170 - ≥ 485 ≥ 40 - - - ≥ 50

MECHANICAL PROPERTIES IN SOLUTION ANNEALED CONDITION (+AT)


AT HIGHER TEMPERATURES ACCORDING TO DIN EN 10088-3

Temperature in °C 100 150 200 250 300 350 400 450 500 550

Rp0.2 in MPa ≥ 165 ≥ 150 ≥ 137 ≥ 127 ≥ 119 ≥ 113 ≥ 108 ≥ 103 ≥ 100 ≥ 98

Rp1.0 in MPa ≥ 200 ≥ 180 ≥ 165 ≥ 153 ≥ 145 ≥ 139 ≥ 135 ≥ 130 ≥ 128 ≥ 127

FORGING COLD FORMING


Acidur 4404 is usually heated slowly to 1150°C - Acidur 4404 is suitable for cold forming according to
1180°C. The temperature range for forging is 900°C DIN EN 10263-5. Modified analysis with better cold
03/06/2016 2016-0036 Page 03

- 1180°C. If no bending is expected, the material is forming behaviour are available on request.
cooled rapidly in water (or air) to avoid undesired
phases which reduce the corrosion resistance and
mechanical properties. Tempering colours and scale
layers reduce the corrosion resistance and must be
removed by pickling or other suitable methods.
Acidur 4404
TECHNICAL DATA SHEET
X2CrNiMo17-12-2
1.4404

CORROSION RESISTANCE WELDING


(PREN = 23.1-28.5)
Acidur 4404 is weldable with or without filler materi-
Due to the molybdenum content of 2% - 2.5% al (e.g. 1.4430). The interpass temperature should
the corrosion resistance (especially in presence of not exceed 200°C. Subsequent heat treatment is not
chorides) is significantly higher than the corrosion required. The resistance to intergranular corrosion is
resistance of Acidur 4301 and Acidur 4307. In most unaffected by welding (acc. to DIN EN ISO 3651 part 2).
natural environmental media and industrial areas with
moderate concentrations of chloride and salt as well as
in the food and pharmaceutical industries, Acidur 4404 STRAIN HARDENING DIAGRAM
shows an excellent corrosion resistance. Due to the 2,000 100
lower carbon content Acidur 4404 is resistant to inter-
1,800 90
granular corrosion in accordance to DIN EN ISO 3651
Yield strength and tensile strength in MPa

part 2 (also after welding). However Acidur 4404 is not 1,600 80

resistant to sea water. 1,400 Z 70

Reduction of area in %
1,200 60

Corrosive Concentration Temperature Resistance 1,000 50


medium
NaCl saturated 20°C risk of 800 40

pitting corrosion 600 Rm


30
Seawater - 20°C risk of
400 20
pitting corrosion Rp0.2
Water varpour - 400°C resistant 200 10
drawn in 4 processing steps from Ø 3.4 to Ø 1.98 mm
Nitric acid 7% 20°C resistant
0 0
Sulphuric acid 1% 20°C resistant 0 10 20 30 40 50 60 70 80 90 100
Formic acid 10 % 20°C resistant Deformation in %

Laboratory experiments with pure corrosive agent and optimal


specimens are the basis of these corrosion resistance tests.
Note: These results are a non-binding indication.
03/06/2016 2016-0036 Page 04
Acidur 4404
TECHNICAL DATA SHEET
X2CrNiMo17-12-2
1.4404

MACHINING

For Acidur 4404 we recommend the following cutting conditions:

CUTTING CONDITIONS

Tool angle

Processing Cutting speed Depth of cut Feed rate Cutting angle Clearance angle Inclination angle
type in m/min in mm in mm/U

Drilling 40 - 100 - 0.05 - 0.16 140° Tip angle 140° Tip angle -

Turning 70 - 175 6 0.1 - 0.5 10° - 16° 6° - 8° -4° and 4°

Milling 125 - 260 - 0.15 - 0.3 - - -

Cutting data can be seen as an indication and are only for an assessment of the processing parameters.
Analysis variants to optimise the machining properties on request.

DELIVERY CONDITIONS
Wire rod Ø 5.5 - 30.0 mm You can find our complete delivery programme
Bars Ø 7.0 - 250.0 mm in the brochure “High-tech Steel Solutions for
Bright steel in bars Ø 2.0 - 290.0 mm Tomorrow’s World (Products and Services)”
Bright steel in coils Ø 0.8 - 20.0 mm on www.dew-stahl.com.

completion: solution annealed, pickled, drawn, forged, rolled,


straightened, peeled and grounded. Dimensions > 290 mm
available after consultation.

We reserve the right to change the content of our technical datasheets without prior notice at any time to remove and/or edit in any way.
Errors and misprints reserved.

Deutsche Edelstahlwerke GmbH


Auestr. 4
03/06/2016 2016-0036 Page 05

58452 Witten
Germany
Phone: +49 (0) 2302 29 - 0
Fax: +49 (0) 2302 29 - 4000

info@dew-stahl.com
www.dew-stahl.com

You might also like