Location via proxy:   [ UP ]  
[Report a bug]   [Manage cookies]                

Ada 311689

Download as pdf or txt
Download as pdf or txt
You are on page 1of 798

WL-TR-94-4053

Volume 2, Chapters 5 and 6

DAMAGE TOLERANT DESIGN


HANDBOOK

D.A. Skinn, J.P. Gallagher, A.P. Berens,


P.D. Huber, J. Smith

University of Dayton Research Institute


300 College Park Dr
Dayton, OH 45469-0120

May 1994
Final Report for Period June 1991 - May 1994

Approved for public release; distribution unlimited

Materials Directorate
Wright Laboratory
Air Force Materiel Command
Wright Patterson AFB, Ohio 45433-7734

19960809 031

THIS DOCUMENT IS BEST


QUALITY AVAILABLE.

THE

COPY FURNISHED TO DTIC


CONTAINED A SIGNIFICANT
NUMBER OF PAGES WHICH DO
NOT REPRODUCE LEGIBLY.

Form Approvod-

REPORT DOCUMENTATION PAGE

MB No. 0704-0188

Public reporting burden for this collection of information is estimated to average 1 hour per response, including the time for reviewing instructions, searching existing data sources
gathering and maintaining the data needed, and completing and reviewing the collection of information. Send comments regarding this burden estimate or any other aspect of thii.
collection of information, including suggestions for reducing this burden, to Washington Headquarters Services. Directorate tor Information Operations and Reports, 1215 Jefferson
Davis Highway Suite 1204, Arlington, VA 22202-4302, and to the Office of Management and Budget, Paperwork Reduction Project (0704-0188), Washington, DC 2050J; "

1. AGENCY USE ONLY (Leave blank)

4. TITLE AND SUBTITLE

2.REPO%DATE1994

3. REPORT TYPE AND DATE,

FINAL

DAMAGE TOLERANT DESIGN HANDBOOK

8.5. FUNDING NUMBERS

C F33615-91-C-5610S
PE'
62102
PR
2418
TA
04
W
91

VOL 2, CHAPTERS 5 AND 6


6. AUTHOR(S)

9105/19/94

D#A# SKINN, J.P. GALLAGHER,


A.P. BERENS, P.D. HUBER,
J. SMITH

\ 7. PERFORMING ORGANIZATION NAME(S) AND ADDRESS(ES)

UNIVERSITY OF DAYTON RESEARCH INSTITUTE


300 COLLEGE PARK

8. PERFORMING ORGANIZATION
REPORTIMUMBER

DAYTON OH 45469-0120
I 10. SPONSORING/MONITORING
AGENCY REPORT NUMBER

9. SPONSORING /MONITORING AGENCY NAME(S) AND ADDRESS(ES)

MATERIALS DIRECTORATE
WRIGHT LABORATORY
AIR FORCE MATERIEL COMMAND
WRIGHT PATTERSON AFB OH 45433-7734

WL-TR-94-4053

| 11. SUPPLEMENTARY NOTES

12b. DISTRIBUTION CODE

12a. DISTRIBUTION/AVAILABILITY STATEMENT

APPROVED FOR PUBLIC RELEASE; DISTRIBUTION IS


UNLIMITED.

13. ABSTRACT (Maximum 200 words)

\
|
i
I

This report presents a compilation of mechanical property data that are useful for
damage tolerant design and analyses. The data of this haiidbodk combines the old
data that were previously presented in MCIC-HB-OIR (Damage Tolerant Design
Handbook, December 1983) and more recent data that were collected from various

I sources.

The fracture toughness, crack growth, R-curve, sustained load and

! threshold data are for alloy and stainless steels, nickel based' super alloys,
\ titanium alloys and aluminum alloys. .
""'"-"' 'i

i 14. SUBJ

ICAL PROPERTIES
FRACTURE TOUGHNESS
SUBCRITICAL CRACK GROWTH

! 17. SECURITY CLASSIFICATION


OF REPORT

UNCLASSIFIED

NSN 7540-01-280-5500

15. NUMBER OF P*

R-CURVES
SUSTAINED LOAD
THRESHOLD

18. SECURITY CLASSIFICATION


OF THIS PAGE

UNCLASSIFIED

16. PRICE CODE

19. SECURITY CLASSIFICATION


OF ABSTRACT -

20. LIMITATION Of ABSTRACT

UNCLASSIFIED

' Standard Form 298 (Rev. 2-89)


Prescribed by ANSI Std."2:39-'i8 ""'"'""
298-102

GENERAL INSTRUCTIONS FOR COMPLETING SF 298

The Report Documentation Page (RDP) is used in announcing and cataloging reports. It is important
that this information be consistent with the rest of the report, particularly the cover and title page.
Instructions for filling in each block of the form follow. It is important to stay within the lines to meet
optical scanning requirements.

Block 1

<

Agency Use Only (Leave blank).

Block 2. Report Date. Full publication date


including day, month, and year, if available (e.g. 1
Jan 88). Must cite at least the year.
Block3. Type of Report and Dates Covered.
State whether report is interim, final, etc. If
applicable, enter inclusive report dates (e.g. 10
Jun87-30Jun88).
Block 4. Title and Subtitle. A title is taken from
the part of the report that provides the most
meaningful and complete information. When a
report is prepared in more than one volume,
repeat the primary title, add volume number, and
include subtitle for the specific volume. On
classified documents enter the title classification
in parentheses.
Block 5. Funding Numbers. To include contract
and grant numbers; may include program
element number(s), project number(s), task
number(s), and work unit number(s). Use the
following labels:
C
G
PE

Contract
Grant
Program
Element

PR
TA
WU

Project
Task
Work Unit
Accession No.

Block 6. Author(s). Name(s) of person(s)


responsible for writing the report, performing
the research, or credited with the content of the
report. If editor or compiler, this should follow
the name(s).
Block 7. Performing Organization Name(s) and
Address(es). Self-explanatory.
Block 8. Performing Organization Report
Number. Enter the unique alphanumeric report
number(s) assigned by the organization
performing the report.
Block 9. Sponsoring/Monitoring Agency Name(s)
and Address(es). Self-explanatory.
Block 10. Sponsoring/Monitoring Agency
Report Number. (If known)
Block 11. Supplementary Notes. Enter
information not included elsewhere such as:
Prepared in cooperation with...; Trans, of...; To be
published in.... When a report is revised, include
a statement whether the new report supersedes
or supplements the older report.

Block 12a. Distribution/Availability Statement.


Denotes public availability or limitations. Cite any
availability to the public. Enter additional
limitations or special markings in all capitals (e.g.
NOFORN, REL, ITAR).
DOD -

DOE NASANTIS -

Block 12b
DOD DOE -

See DoDD 5230.24, "Distribution


Statements on Technical
Documents."
See authorities.
See Handbook NHB 2200.2.
Leave blank.

Distribution Code.
Leave blank.
Enter DOE distribution categories

from the Standard Distribution for


Unclassified Scientific and Technica
Reports.
NASA- Leave blank.
NTIS - Leave blank.
Block 13. Abstract. Include a brief (Maximum
200 words) factual summary of the most
significant information contained in the report.
Block 14. Subject Terms. Keywords or phrases
identifying major subjects in the report.
Block 15. Number of Pages. Enter the total
number of pages.
Block 16. Price Code. Enter appropriate price
code (NTIS only).
Blocks 17.-19. Security Classifications. Selfexplanatory. Enter U.S. Security Classification in
accordance with U.S. Security Regulations (i.e.,
UNCLASSIFIED). If form contains classified
information, stamp classification on the top and
bottom of the page.
Block 20. Limitation of Abstract. This block must
be completed to assign a limitation to the
abstract. Enter either UL (unlimited) or SAR (same
as report). An entry in this block is necessary if
the abstract is to be limited. If blank, the abstract
is assumed to be unlimited.
Standard Form 298 Back (Rev. 2-89)

* U.S.GPO: 1990-0-273-271

Table of Contents
VOLUME 1
Chapter
1

Page
Handbook Organization and Content

1-1

1.0

Overview

1-1

1.1

Organization

1-2

1.2

Data Ordering and Abbreviations


1.2.1 Sorting Order
1.2.2 Abbreviations

1-5
1-5
1-5

1.3

Material Chapter Summaries


1.3.1 Available Data Summary
1.3.2 Plane Strain Fracture Toughness Material
Data Summary
1.3.3 Plane Stress and Transitional Fracture Material
Data Summary
1.3.4 Fatigue Crack Growth Rate Material Data
Summary
1.3.5 Stress Corrosion Cracking Threshold Material
Data Summary

1-19

1.4

Alloy Section Summaries

1-21

1.5

Alloy
1.5.1
1.5.2
1.5.3

Fracture Toughness Subsection Formats


Plane Strain Fracture Toughness Data
Plane Stress Fracture Toughness Data
R-Curve Data

1-23
1-25
1-25
1-29

1.6

Subcritical Crack Growth Subsection Formats


1.6.1 Fatigue Crack Growth Rate Data
1.6.2 Sustained Load Crack Growth Rate
1.6.3 Stress Corrosion Cracking Threshold

1-29
1-31
1-36
1-38

Methods of Calculation
2.0

1-5
1-12
1-12
1-15
1-15

2-1

Overview
2.0.1 Data Review and Acceptance Criteria
2.0.2 Fracture Mechanics Basis
2.0.3 Test Specimen Geometries
1U

2-1
2-1
2-3
2-4

2.1

Plane-Strain Fracture Toughness (Klc)

2-12

2.2

Critical Plane Stress Fracture Toughness


2.2.1 Plane Stress and Transitional Fracture
Toughness
2.2.2 Plane Stress and Transitional Fracture
Toughness Testing
2.2.3 Critical Stress-Intensity Factor (K,)

2-20

2-23
2-23

2.3

The Apparent Fracture Toughness

2-26

2.4

R-Curve (KR Versus Aaeff)

2-26

2.5

Fatigue Crack Growth Rate


2.5.1 Fatigue Crack Growth Behavior
2.5.2 Data Acceptance Criteria
2.5.3 Data Reduction Procedures
2.5.4 Data Reporting Procedures

. 2-30
2-30
2-32
2-33
2-35

2.6

Sustained-Load Crack Growth Rates


2.6.1 Sustained-Load Crack Growth Behavior
2.6.2 Data Acceptance Criteria
2.6.3 Data Reduction Procedures
2.6.4 Data Reporting Procedures

2-38
2-38
2-40
2-40
2-40

2.7

Threshold Stress Intensity (KIscc)


2.7.1 The Threshold
2.7.2 Conditions for Validity of Data

2-41
2-41
2-43

Alloy Steel Sections


3.0

Alloy
3.0.1
3.0.2
3.0.3
3.0.4
3.0.5

3.1
3.2
3.3
3.4
3.5
3.6
3.7
3.8
3.9
3.10

lONi Steel
12-9-2(MAR)
12Ni-5Cr-3Mo
18Ni(180)(MAR)
18Ni(200)(MAR)
18Ni(250)
18Ni(250)(MAR)
18Ni(280)(MAR)
18NK300)
18Ni(300)(MAR)

2-20

3-1

Steel Material Summaries


Available Data Summary
KIc Summary
K,. Summary (Without Buckling Constraints)
FCGR at Defined AK Levels
KIscc Summary

3-3
3-3
3-20
3-27
3-28
3-33
3-39
3-48
3-51
3-52
3-53
3-56
3-59
3-67
3-68
3-70

iv

3.11
3.12
3.13
3.14
3.15
3.16
3.17
3.18
3.19
3.20
3.21
3.22
3.23
3.24
3.25
3.26
3.27
3.28
3.29
3.30
3.31
3.32
3.33
3.34
3.35
3.36
3.37
3.38
3.39
3.40
3.41

18NK350)
18Ni(350)(MAR)
300M
300M(AM)
300M(VAR)
300MCVM)
4140
4330V
4330V(MOD)
4340
4340(AM)
4340(DH)
4340(EFM)
4340(MOD)
4340(VAK)
4340V
A286
AF1410
AF1410(VIM-VAR)
D6AC
Hll
HP9-4-.20
HP9-4-.20(CEVM)
HP9-4-.25(VAE)
HP9-4-.30
HP9-4-.45
HY-150
HY-180
HY-80
HY-TUF
Alloy Steel References

Stainless Steel Sections

3-88
3-89
3-90
3-134
3-136
3-138
3-140
3-143
3-144
3-149
3-194
3-196
3-198
3-199
3-200
3-202
3-204
3-212
3-222
3-233
3-300
3-308
3-348
3-354
3-356
3-423
3-424
3-425
3-428
3-431
3-433
4-1

4.0

Stainless Steel Material Summaries


4.0.1 Available Data Summary
4.0.2 KIc Summary
4.0.4 FCGR at Defined AK Levels
4.0.5 KIscc Summary

4-3
4-3
4-9
4-11
4-15

4.1
4.2
4.3
4.4
4.5
4.6
4.7
4.8

15-5PH
15-5PH(AM)
15-5PH(VM)
17-4PH
17-7PH
21-6-9 NI40
304
316

4-17
4-47
4-48
4-49
4-61
4-69
4-72
4-86

4.9
4.10
4.11
4.12
4.13
4.14
4.15
4.16
4.17
4.18
4.19
4.20

347
AFC 260
AFC 77
AFC 77(VAR)
AM 355
AM 362
AM 364
CUSTOM 455
PH13-8MO
PH14-8MO
PH15-7Mo
Stainless Steel References

4-92
4.97
4.98
4-103
4-106
4-107
4-108
4-109
4-119
4-193
4-194
4-197

VOLUME 2
5

Nickel Based Super Alloys Sections


5.0

5.1
5.2
5.3
5.4
5.5
5.6
5.7
5.8
5.9
5.10
5.11
5.12
5.13
5.14
6

Nickel Based Super Alloys Material Summaries


5.0.1 Available Data Summary
5.0.2 KIc Summary
5.0.3 K,. Summary (Buckling not Constrained)
5.0.4 FCGR at Defined AK Levels
5.0.5 KIscc Summary
ASTROLOY 901
ASTROLOY P/M-H
ASTROLOY P/M-W
IN100
IN100 P/M-G
INCOLOY 901
INCONEL 600
INCONEL 625
INCONEL 718
NASA IIB-7 P/M
P/M RENE 95
RENE 95 (H&F)
WASPALOY
Nickel Based Super Alloys Reference

Titanium Alloys Sections


6.0

5-1
5-3
5-3
5-6
5-7
5-8
5-12
5-13
5-24
5-26
5-28
5-52
5-54
5-56
5-63
5-68
5-162
5-163
5-170
5-171
5-198
6-1

Titanium Alloys Material Summaries


6-3
6.0.1 Available Data
6-3
6.0.2 KIe Summary
6-15
6.0.3.1 K,. Summary (Buckling not Constrained) .... 6-18
6.0.3.2 K, Summary (Buckling Constrained)
6-19
6.0.4 FCGR at Defined AK Levels
6-20
6.0.5 KIscc Summary
6-35

vi

6.1
6.2
6.3
6.4
6.5
6.6
6.7
6.8
6.9
6.10
6.11
6.12
6.13
6.14
6.15
6.16
6.17
6.18
6.19
6.20
6.21
6.22
6.23
6.24
6.25

BETA
BETA C
BETA III
BETA Ti
CORONA 5
IMI-834
Ti-*
Ti-10-2-3
Ti-4Al-3Mo-lV
Ti-5-2.5 ELI
Ti-5Al-2.5Sn
Ti-6-2-2-2-2
Ti-6-2-4-2
Ti-6-2-4-2 ELI
Ti-6-2-4-6
Ti-6A1-4V
Ti-6A1-4V ELI
Ti-6Al-6V-2Sn
Ti-6Al-6V-2.5Sn
Ti-6A12Sn4Zr6Mo
Ti-8Al-lMo-lV
Ti-Mo8V2Fe3Al
Ti-5A12.5Sn ELI
Ti-6A16V2Sn ELI
Titanium Alloys References

6-38
6-39
6-47
6-59
6-61
6-62
6-68
6-69
6-72
6-73
6-102
6-126
6-134
6-141
6-154
6-169
6-433
6-473
6-515
6-516
6-518
6-567
6-569
6-571
6-573

VOLUME 3
7

Aluminum 2000/6000 Series Alloys Sections

7-1

7.0

Aluminum 2000/6000 Series Material Summaries


7-3
7.0.1 Available Data
7-3
7.0.2 KIc Summary
7-8
7.0.3.1 K, Summary (Buckling not Constrained) .... 7-10
7.0.3.2 K, Summary (Buckling Constrained)
7-12
7.0.4 FCGR at Defined AK Levels
7-13
7.0.5 KIscc Summary
7-25

7.1
7.2
7.3
7.4
7.5
7.6
7.7
7.8
7.9

2014
2020
2020 (ALCLAD)
2021
2024
2024 (ALCLAD)
2048
2091
2124

7-27
7-65
7-78
7-79
7-82
7-378
7-397
7-416
7-451

Vll

7.10
7.11
7.12
7.13
7.14
7.15
7.16
7.17
7.18
7.19
7.20

2214
2219
2324
2419
2618
6061
A201
A357
AL905XL
IN905XL
Aluminum 2000/6000 Series References

7-556
7-561
7-654
7-657
7-668
7-674
7-682
7-686
7-691
7-704
7-719

VOLUME 4
8

Aluminum 7000/8000 Series Alloys Sections

8-1

8.0

Aluminum 7000/8000 Series Material Summaries


8-3
8.0.1 Available Data
8-3
8.0.2 KIc Summary
8-12
8.0.3.1 K^ Summary (Buckling not Constrained) .... 8-16
8.0.3.2 K,. Summary (Buckling Constrained)
8-19
8.0.4 FCGR at Defined AK Levels
8-20
8.0.5 KIscc Summary
8-41

8.1
8.2
8.3
8.4
8.5
8.6
8.7
8.8
8.9
8.10

7001
7005
7007
7010
7039
7049
7050
7050 (ALCLAD)
7075
7075 (ALCLAD)

8-45
8-53
8-62
8-63
8-80
8-81
8-136
8-435
8-452
8-745

7079
7079 (ALCLAD)
7080
7149
7150
7175
7178
7178 (ALCLAD)
7475
7475 (ALCLAD)

8-766
8-833
8-836
8-837
8-849
8-877
8-969
8-1019
8-1020
8-1292

VOLUME 5
8.11
8.12
8.13
8.14
8.15
8.16
8.17
8.18
8.19
8.20

vm

8.21
8.22
8.23
8.24
8.25

8009
8090
X7090
X7091
Aluminum 7000/8000 Series References

IX

8-1323
8-1328
8-1344
8-1348
8-1354

Foreword
This report summarizes the results of a damage tolerant, material property data
collection and reporting program conducted under USAF Contract F33615-91-C-5610.
The work was sponsored by the Materials Directorate of Wright Laboratory with Mr.
Jack Coate of the Systems Support Division serving as the project monitor. The
technical effort was conducted between June 1991 and January 1994. The work was
performed by the University of Dayton Research Institute under the general
supervision of Dr. Joseph P. Gallagher with Dr. Alan P. Berens serving as Principal
Investigator.
This final report comprises eight chapters which are presented in five volumes
as follows:
VOLUME

CHAPTER

Handbook organization and content

Methods of calculation

Alloy Steels

Stainless Steels

Nickel Based Super Alloys

Titanium Alloys

DESCRIPTION

Aluminum 2000/6000 Series Alloys


4&5

Aluminum 7000/8000 Series Alloys

A detailed listing of the materials represented in the Handbook is contained in


the preceding Table of Contents.

In the body of the Handbook, the pages are

numbered within chapters and the relevant portion of the table of contents is
repeated at the beginning of each chapter.

XL

CHAPTER 5
NICKEL BASED SUPER ALLOYS SECTIONS
5.0
5.0.1
5.0.2
5.0.3.1
5.0.4
5.0.5
5.1
5.2
5.3
5.4
5.5
5.6
5.7
5.8
5.9
5.10
5.11
5.12
5.13
5.14

Nickel Based Super Alloys Material Summaries


Available Data Summary
Klc Summary
K,. Summary (Buckling not Constrained)
FCGR at Defined AK Levels
Kj.ee Summary
ASTROLOY901
ASTROLOY P/M-H
ASTROLOY P/M-W
IN100
IN100 P/M-G
INCOLOY901
INCONEL600
INCONEL 625
INCONEL 718
NASA HB-7 P/M
P/M RENE 95
RENE 95 (H&F)
WASPALOY
Nickel Based Super Alloys References

5-1

5-3
5-3
5-6
5-7
5-8
5-12
5-13
5-24
5-26
5-28
5-52
5-54
5-56
5-63
5-68
5-162
5-163
5-170
5-171
5-198

u
o

ta

W
w

73

13

to

00

00

CO

CO

e*

CO

kO

US

be

ffl

&

01

CO

a
E

10

"d

>
J*
0

ti
V

M
o
I

roduc
Form

-W

cu

"8
IS
g.

bo

bo

c
*S>

Jo
Q

IG

'S
4>

'S
E

bo

be

bo
ft

&

fa

fa

<

<

as
X

onditic
t Treat

00

'S

c
3

fao
8

<

OS
X

<

<

l>
CD

fa

13

i
is

to

88
0)

8
O

fa
8

io

m
a
3

c
3

C-;

fa
$
to

<

8
S

s.

c
D

fa
o

l-H

>
S

1<

>
3

B
<

><

2
o
B
<

1o
o

03

s
&

i8r>
-<

Is
g=

fa
s
CO

<

a:

fa
S

f?

fa

fa
ao

o
01

as
o
IS

CO

S
o

IN

00

BS

o
Oi

>
S

o
o
2

CO

fa

LO
CM
CO
J

00

CO
J

5-3

o
Z

fa
s

<

u
u
00

IO

m
"S3
ns

to

IO

"e3

i>

*r

00

>
h
0

tf
u

10

tt

c-

^"

be
C

to
ca

roduc
Form

Jo

bo
C

'&

a
S3

'S

fi?

s
CO

0
a

&

O
a
c
3
0
K

C
3
O
05

bo
C

&

<

fa

&.

<

<

1
c
D

bo
c
&

.1

Q*
a

<

dition/
reatment

id

CH

IS

0
i

<

H
i

is is
as
go
fe OS

fa BS

-or s0

1fa

OS ""
X

fa
8
tr-

en
05
X
GO

u
fa u
3 j

ES
8
t

ft. =>
8
Of

fa

fc
c

Cu

<

A*"?2

cs

fa
0
0
N

s5
6.
0
CO
W

fa

fa

fa

fa
S
00

*"

63

&- M
0 .
1-. 0

5
w
a.
0
a
n
OS

j
0

t*

fa

&.

0
m

fc.
s

CO

&

<

fa

fa

fa
s

5-4

<:

g
0

CO

as

en

Of

s
<
<
Z

W c

OS
X

CN

5
a.

CO

>>
0

TT8

35
u a
#3
80

fa
s03

<

CO

oS

<

fa
to

a
z

<
fa

<

CO

cr

x
Id

ao b.

fa
8

8
*S

%c

fa
C4

CN

to
en

fa
8

>*
a.
en

13

13
0)
>

IG

Condition/
Heat Treatment

Product
Form

>>

0)

JO

CO

X
V

&,
o
CO

a
u
z

5 s

CO

BJ
X

s
s
CO
CO

8
00

<
CO

u.
o
\n
ID

i
in

CO

so
b.
o
w

Ek.
o
o

CO

us
t>
CO

CO

to

GO

&.
o

00

>

So

en U

5-5

"a

a
c

a
02

5s

O
1

c
o

ti

e o >d

0.

9
afi
eo *"

ft

fe?

"0
aa

-u

0)

Min
Spec
Thk

i a

a
a

CO

et

.3 o "3

3 0>C
CO H

t.

aa
c!5 *

aISA'}

bana

s3 0 U
a

^
8

l*g
-w

be

o o
h b
CU

-a
r?

-w

1o s
53 3

fe

a H
o *
ea
Qi

ffl
CO

>>

o
1-H

c-

_:
o

5-6

-t

53

>

<p

"fl

r>

C8

(5
>

B9) *

55

CO

a.

N
to

e
a.

CO

03

CO
C

03
O
10

CD

ua

en

g
CN

CO

IO

so

lO

OS

00

00

CN

CN

o
ed

2 %Q

cc

Yie
tren
(Ks

to

3.

pa

o>
to

CO

s
S

'S

42

a
co

fa

F-

J>

Jl

Ji

^
ffl

o
* ft-.
r* ffl

*J

10 Sa
.d

fci

SH

U 03

CM

CM

o
u
o

<

Q
2

<
*
o

3J

o
a
J
o
u

co

>>
o

C-

o
z

5-7

O
to

3
3

5-8

o
CO

lii

13

Cd

BS

CO

5-9

CO

e
10

5-10

9
s-/

SWS

I
C-.
IS

o
6

h:

CO
CQ

<n
Q

CQ

III

to

a
o

%
GO
OS

BS

2
Et.

cy
OS

z
o

<
X

Iz
J
Ed

J5
O

Ed

5-11

-"

0)

Propellan
Grade
Hydrazin

*a

t>
00

^-

"J a a
C

&.

00

2 j? as B
U

88*8
::-w-:

>

ESHOLD DA
TEMPERAT

SB

hop
aning
Ivent

Sump
Tank
Water

CO

S^
HO

CO
CO

CO
05

J
H

CO

1-1

<N
to
CM
rH

Bpecime
rientati

6-t1

i
i
i

-o

Product
Form

03

CD
<U

s>
bo
s-

CO

fa

s
OJ

fa
o
o

a
fa

Condition/
at Treatment

H
CO H

<u

<N

C o

CO H

STRES
FOR NIC

IS

IONCRACKIN
ALLOYS ATR

jO

03

4>

tN

o
'fa

co
OS

B
03
fa

OS
B
oo o
fa <!

CO "5

-5

S3

0>r1

tt SO

1880F IHR A

f
1

.'*

MartinMarietta
fined Grade
-lydrazine

athe
ema
%G
ydra

OS
B

fa
o
m
CO
!-H

00
i

>>
o
^
<:

ca
"Z
o

5-12

ASTROLOY901

US?
!

V->

IS*

tN

s
3

05

w
cu

5-13

EF

I ASTROLOY 901
Condition/Ht:
Form:
Specimen Type: SENT
Orientation:
Stress Ratio: 0.1

Yield Strength:
Ult. Strength:
Specimen Thk: 0.121 - 0.126 in.
Specimen Width: 2.5 in.
Ref: PW003
(1 of 5)

AK (MPaVin)
V-

4
10
' I ' I'M

40
100
1 I I I INI

-1

Environment: Lab Air; 80T

- I

' I TIM

40

100
_L

' I M'l'l

-3
10

o^10-4

\
c
_

z 10

"o
_K r10

10

10

10
10
-2-r,
O

o 10
10"3
,-s

Z10

10

-o

10
10

10
10

IQ-f

I i I, I
4

10
10

40

"

-z: 10

_rtD

25.
30.
35.
40.
50.
59.15 (max)

m^

.8

o
-3 |

-zz 10

Jio

>
T7

-zz 10

-zz 10

, I,I,I,

1 , 1,1,1,

10

40

100

1.25

da/dN (10"6in/cycle)
1.94
3.60
7.09
12.1
18.8
27.4
51.3
88.1
167.
393.
948.

16.50 (min)
20.
25.
30.
35.
40.
50.
60.
70.
80.
88.23 (max)

Life Prediction Ratio Summary


.5

JP
&

AK (KsiVin)

0.841
1.11
2.62
4.44
6.59
9.30
18.3
35.9

18.88 (min)
20.

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

-z: 10"2

</

100

f
1

AK (KsiVin)

12.50

10

Environment: Lab Air; 800T

10

10

RMS s
Error

(2 of 5)

AK (MPaVin)

i-'

2.

RMS %
Error
21.01

Figure 5.1.3.1.1
' 5-14

Life Prediction Ratio Summary


0.

.5

.8

1.25

ASTROLOY 901
Condition/Ht:
Form:
Specimen Type: SENT
Orientation:
Stress Ratio: 0.1

Yield Strength:
Ult. Strength:
Specimen Thk: 0.121 - 0.126 in.
Specimen Width: 2.5 in.
Ref: PW003
(3 of 5)

AK (MPaVin)
4

I- I

10

' I 'I'l'l

EF

40
100
-ii i i i nil

Environment: Lab Air; 950F

(4 of 5)

AK (MPaVin)
10

40

100

= i ' i M'l'irI ' I 'I'l'l

Environment: Lab Air; 1100F 10

10
10

-3

10

o
u10"

T>

10

-6

10

10

10
4

10

40

100

AK (KsiVin)

16.
20.
25.
30.
35.
40.
50.
60.
70.
71.72 (max)

.5

.8

100

da/dN (10"6in/cycle)
7.56
11.5
19.7
27.6
36.2
46.5
79.0
145.
241.

25.
30.
35.
40.
50.
60.
67.44 (max)

Life Prediction Ratio Summary


i

40

17.59 (min)
20.

2.63
3.28
6.29
10.8
16.4
23.4
32.8
63.5
124.
249.
281.

14.98 (min)

RMS %
Error
20.98

AK (KsiVin)

da/dN (10-6in/cycle)

AK (KsiVin)

10

AK (KsiVin)

1.25

RMS %
Error
14.54

Life Prediction Ratio Summary

Figure 5.1.3.1.1 (Continued)


5-15

r~

.8

1.25

EF

I ASTROLOY 901
Condition/Ht:
Form:
Specimen Type: SENT
Orientation:
Stress Ratio: 0.1

Yield Strength:
Ult. Strength:
Specimen Thk: 0.121 - 0.126 in.
Specimen Width: 2.5 in.
Ref: PW003
(5 of 5)

AK (MPaVin)
1

- I

10

40

' I M'l'l

AK (MPaVin)
4

100

' I 'ITI

- I

-*-

10

' I M'l'l

40

100

' I M'l'l

Environment: Lab Air; 1350T

10

10
-

10

10
10
10
_0)

2 10

"u

_c

10

10

"

I , I,I,I,

I I I,I,I,

40

10

RMS %
Error

10
10
10

10
4

100

da/dN (10"Mn/cycle)

.5

.8

10

40

100

AK (KsiVin)

Life Prediction Ratio Summary


0.

10

AK (KsiVin)
AK (KsiVin)

_*T>

10

10

-3 |

10

Z 10

10

10

o
6-10-4
\
c
_

da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error

Life Prediction Ratio Summary

1.25

0.

2.

Figure 5.1.3.1.1 (Concluded)


5-16

.5

.8

1.25

This page intentionally left blank

5-17

EF

I ASTROLOY 901
Condition/Ht:
Form:
Specimen Type: SENT

Yield Strength:
Ult. Strength:
Specimen Thk: 0.12 - 0.124 in.
Specimen Width: 2.5 in.
Ref: PW003

Orientation:
Stress Ratio: 0.5

(1 of 3)

AK (MPaVin)
4

10

I | l|l|'|

40

100

I | 'I'l'l

10

10

&
o

10

10

10"

q;

_a)

O-10~~

10

Z. 10

10

Jio
>

2:
-= 10 '\
u
x>

PI

10

ii

10"

i "n

T3

o 10

10

10
10

10

-n 10

10
10

_L

' I 'I'l'l

-3

"~"

10

' I 'I'l'l

100

10

10

40

10

10

_Q3

10

Environment: Lab Air; 950T

10

Environment: Lab Air; 800F

(2 of 3)

AK (MPaVin)

" I , LI,I,
4

I , I,I,I,

10

40

10

- i , 1.1,i,
4

100

da/dN (1CT6in/cycle)

RMS %
Error
15.77

.5

.8

1.60
4.57
10.0
15.6
20.7
27.7
39.7
50.9

13.38 (min)
16.
20.

25.
30.
35.
40.
42.89 (max)

Life Prediction Ratio Summary


0.

100

da/dN (10"6in/cycle)

AK (KsiVin)

1.27
1.31
2.34
3.65
5.91
9.79
15.2
22.7
32.9
59.3

9.87 (min)
10.
13.
16.
20.
25.
30.
35.
40.
48.57 (max)

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , l.l.l,

10

1.25

RMS %
Error
16.54

Figure 5.1.3.1.2
5-18

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

i--

2.

-. I

10

(3 of 3)

40

AK (MPaVin)
1

100

4
_

10

| , ,,|,|

40
|

100

| ,,,,,,

_t

ID"3

10
io"3

io"2
o

o
6^10-+
\
c
-^

in1

,n-P

iffj

2T

zio"5

-z.

m
a

T3

10 \
a
a

-6
10

<D

"""

QJ

o
u 10
\
c
^-^
zio"5
a
\
o
" -6
10

I , 1,1,1,

I , I,I,I,

10

40

RMS %
Error
13.77

-z.
>
D

-5

~~ 10

io'7

-6

10

m"8

- I , I,I,I,
1

100

I < I.I,I,

10

40

100

AK (KsiVin)

da/dN (10~6in/cycle)

15.58 (min)
16.
20.
25.
30.
35.
40.
48.57 (max)

E
-'

"O

AK (KsiVin)
AK (KsiVin)

10

10

10

"

-6

in*

1(f

zz

-s

10
io"7

io"2

QJ

<D

\
D
"

10

Environment: Lab Air; 1100F 10


"~~
_
-1

"" 10

ID"2

Yield Strength:
Ult. Strength:
Specimen Thk: 0.12 - 0.124 in.
Specimen Width: 2.5 in.
Ref: PW003

AK (MPaVin)
4

EF

Condition/Ht:
Form:
Specimen Type: SENT
Orientation:
Stress Ratio: 0.5

in -i

ACTDni nv

da/dN (10"6in/cycle)

AK (KsiVin)

5.41
5.92
11.5
19.4
27.7
36.3
49.6
124.

Life Prediction Ratio Summary


i

0.

.5

.8

i"

1.25

RMS x
Error

Life Prediction Ratio Summary

0.

2.

Figure 5.1.3.1.2 (Concluded)


5-19

.5

.8

1.25

2.

EF

I ASTROLOY 901
Condition/Ht:

Yield Strength:
Ult. Strength:
Specimen Thk: 0.119 - 0.123 in.
Specimen Width: 2.5 in.
Ref: PW003

Form:
Specimen Type: SENT
Orientation:
Stress Ratio: 0.7

(1 of 2)

AK (MPaVin)
4
10
f=li I i Ml'

4
10
i l i i 111

40
100
-ii I i I i|i|

Environment: Lab Air; 800F

(2 of 2)

AK (MPaVin)
40
100
I I I I IMI

Environment: Lab Air; 1100F

10

10

o
\
-3 |

10

10

10

10

10

40

100

RMS %
Error
14.87

6.11
7.65

Life Prediction Ratio Summary


i

.5

.8

100

0.560
0.661
0.894
1.12
1.82
2.78
5.32
14.3

7.57 (min)
8.
9.
10.
13.
16.
20.
25.
25.23 (max)

0.399
0.472
0.594
1.26
2.30
3.86

8.01 (min)
9.
10.
13.
16.
20.
25.
26.83 (max)

40

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (10_6in/cycle)

AK (KsiVin)

10

AK (KsiVin)

AK (KsiVin)

1.25

RMS %
Error
16.94

Figure 5.1.3.1.3
5-20

15.0

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

ASTROLOY 901
Condition/Ht:
Form:
Specimen Type: SENT
Orientation:
Stress Ratio: 0.8

Yield Strength:
Ult. Strength:
Specimen Thk: 0.117 in.
Specimen Width: 2.5 in.
Ref: PW003
(1 of 1)

AK (MPaVin)
4

10

40

AK (MPaVin)
4
10
I I I I I Ml

100

40

100

' I TIM^
10

10

Environment: Lab Air; 950F

10

10

10

10

-3

10

10
2
io"

o
^10"

10"

-3 |

10

d>

_a)
_
o
_
6^10-4

o
\

EF

10"

o
\

'1
s

-^

:
10

10

m~ ^
u

"o

10

- -

"o

XI

10

_K

-5

10

10

10

10

10

10

10

I , I,I,I,
4

10

i I 111li
40

10

100

I Mill
4
10

da/dN (10"6in/cycle)

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


-i

0.

100

1.16
1.52
2.05
3.08
4.86
8.10
12.7

8.44- (min)
9.
10.
13.
16.
20.
24.05 (max)

RMS %
Error
15.00

I I I 111

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

.5

.8

1.25

RMS %
Error

i-'

Life Prediction Ratio Summary


i

0.

2.

Figure 5.1.3.1.4
5-21

.5

.8

1.25

2.

i1 ASTROLOY 901
tr

Condition/Ht:
Form:
Specimen Type: SENT
Orientation: C-R
Stress Ratio: 0.5

Yield Strength:
Ult. Strength:
Specimen Thk: 0.122 in.
Specimen Width: 2.5 in.
Ref: PW003

(1

AK (MPaVin)
1

10

40

10

10"2
10
^^

10

\
c

v_x

10

E
*'

-1

10

io"2^

o
\

o 10
\

10

\
O

\
o

XI

"O

10

- "1,1 .1,1,
1

I , I , 1.1,

10

40

-5

10"7
-6
1

0
iff8

~
1

100

I , I, I,I,

I , I,l,l,

40

da/dN (10"6in/cycle)

10.86 (min)
13.
16.
20.
25.
30.
35.
40.
45.80 (max)

RMS %
Error
11.88

.5

.8

-6

10

100

1.25

da/dN (10"6in/cycle)

AK (KsiVin)
11.04 (min)
13.
16.
20.
25.
30.
35.
36.86 (max)

1-84
2.55
3.77
5.94
9.75
14.3
19-8
28.5
38.4

Life Prediction Ratio Summary


0.

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

>
xs

~~n 10

10

10"7

10

-6

-5

^"'

Z10"5

2 10-5
TJ

10

100

<D
O

40

2)

io-3

__

10

-1

- I I | t'l
I ' I ' ITI
-1
0
Environment: Lab Air; 1100F 10

ID"3

(2

AK (MPaVin)

2)

100

Environment: Lab Air; 800T


ID"2

2.

RMS %
Error
16.45

Figure 5.1.3.1.5
5-22

3.90
5.89
9-84
16.7
26.5
32.7
37.9
42.0

Life Prediction Ratio Summary


0.

.5

.8

1.25

2.

This page intentionally left blank

5-23

ASTROLOY P/M-H
Condition/Ht: 2025F 3HR AC 1600F 8HR AC
Form: Disk
Specimen Type: WOL
Orientation: C-R
Stress Ratio: 0.05
Environment: LAB AIR;1200F
(1 of 4)

AK (MPaVin)
4

10

(2 of 4)

AK (MPaVin)
4

40
100
I I 11II

= I ' I 'IT

Yield Strength: 135.8 ksi


Ult. Strength: 202 ksi
Specimen Thk: 0.5 in.
Specimen Width: 2.5 in.
Ref: PW004

10

40
100
i Minn

Frequency: 0. Hz

10

10
o
6^10-4

10

10

10

10
4

10

40

100

AK (KsiVin)

25.
30.
35.
40.
50.
60.
70.
80.
90.
93.51 (max)

RMS %
Error
66.39

Life Prediction Ratio Summary


0.

.5

.8

100

14.1
17.2
30.7
59.1
108.
258.
411.
607.
1019.
1022.

21.63 (min)
25.
30.
35.
40.
50.
60.
70.
80.
80.05 (max)

61.8
61.8
71.6
94.6
132.
262.
492.
845.
1326.
1913.
2136.

23.79 (min)

40

da/dN (10-6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

10

AK (KsiVin)

1.25

RMS %
Error
35.81

Figure 5.2.3.1
5-24

Life Prediction Ratio Summary


0.

.5

.8

1.25

2.

ASTROLOY P/M-H
Condition/Ht: 2025F 3HR AC 1600F 8HR AC
Form: Disk
Specimen Type: WOL
Orientation: CR
Stress Ratio: 0.05
Environment: LAB AIR;1200F

10

Yield Strength: 135.8 ksi


Ult. Strength: 202 ksi
Specimen Thk: 0.5 in.
Specimen Width: 2.5 in.
Ref: PW004

(3 of 4)

AK (MPaVin)

- i 'i M'l'ir

(4 of 4)

AK (MPaVin)
1

40
100
-ii | i I iiil

b I

10

' I Tl'l

40

100

' I M'l'l

-H

10

Frequency: 0.33 Hz
10

10
10
_a>
o

o 10
- 10" E

10

-AT)
10

T3

10
10
10
10

10
4

10

40

100

AK (KsiVin)
da/dN (10-6in/cycie)

AK (KsiVin)

35.
40.
50.
60.
62.12 (max)

RMS %
Error
25.09

Life Prediction Ratio Summary


0.

.5

.8

40

100

1.25

da/dN (10"6in/cycle)

AK (KsiVin)

2.38
2.63
4.53
8.25
13.5
20.2
27.9
35.4

15.27 (min)
16.
20.
25.
30.
35.
40.
44.64 (max)

2.67
3.95
7.93
14.9
24.2
35.7
49.4
84.4
130.
142.

14.25 (min)
16.
20.
25.
30.

10

AK (KsiVin)

2.

RMS %
Error
8.69

Life Prediction Ratio Summary

Figure 5.2.3.1 (Concluded)


5-25

0.

.5

.8

1.25

\ ASTROLOY P/M-W
Condition/Ht: 2025F 4HRS AC
Form: Disk
Specimen Type: WOL
Orientation: CR
Stress Ratio: 0.05
Environment: LAB AIR;1200F

(1 of 3)

AK (MPaVin)
4

10

i- I ' I Tl'l

40
-II

1600F 8HRS AC
Yield Strength: 153 ksi
Ult. Strength: 220 ksi
Specimen Thk: 0.5 in.
Specimen Width: 2.5 in.
Ref: PW004
(2 of 3)

AK (MPaVin)
4

100

10

40

I 11 llll

100

' I TIM

10

Frequency: 0. Hz

10
10
10

o 10

10

10
10
"c

XI

_R -

10
10

10
-6

10
10

i i i 111

10

40

100

AK (KsiVin)
da/dN (10"6 in/cycle)

AK (KsiVin)

RMS %
Error
>100.0

.5

.8

100

2.98
3.29
5.65
10.6
20.6
35.2
54.9
79.4
140.
208.
221.

12.48 (min)
13.
16.
20.
25.
30.
35.
40.
50.

60.
61.82 (max)

Life Prediction Ratio Summary


0.

40

da/dN (10'6in/cycle)

AK (KsiVin)

18.4
21.0
49.5
114.
220.
371.
571.
1162.
2199.
4749.
14463.
30958.

15.46 (min)
16.
20.
25.
30.
35.
40.
50.
60.
70.
80.
84.92 (max)

10

AK (KsiVin)

1.25

RMS %
Error
1 6.04

Figure 5.3.3.1
5-26

Life Prediction Ratio Summary


0.

-r-

T-

.5

.8

1.25

H ASTR0L0Y P/M -Vw*


1600F 8HRS AC
Yield Strength: 153 ksi
Ult. Strength: 220 ksi
Specimen Thk: 0.5 in.
Specimen Width: 2.5 in.
Ref: PW004

Condition/Ht: 2025F 4HRS AC


Form: Disk
Specimen Type: WOL
Orientation: C-R
Stress Ratio: 0.05
Environment: LAB AIR;1200F

(3 of 3)

AK (MPaVin)
1

10

40

AK (MPaVin)
1

100
10

Frequency: 20. Hz

1
.
' F

10

= i i i'i'i

40

100

i 'I'n

10

io"2

10"2
-1

10

10
1_v

io-3

~"

_2

io
o

io~3

/^~\
2

io"

Q3

_jp
jf&

~s

Z10"5
XI

\
o
~

o^10\
c
^-^

\
c

w
m

-6
10

10

10

-z.

2M0-5
XI
10

>
X)

\
o
"

10

10

>
XI

-6 ~
-5

-5

10

10

io"7

io"7

-6

-6

10

10
.^

E
"'

"1,1 ,1,1.
1

I , I,I,I,

10

40

100

da/dN (10"6in/cycle)

16.61 (min)
20.
25.
30.
35.
40.
45.34 (max)

RMS %
Error
16.00

40

100

6
da/dN (10 ~ in/cycle)

AK (KsiVin)

2.54
3.51
5.80
9.19
13.6
18.9
25.1

Life Prediction Ratio Summary


0.

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , I,I,I,

" I , I,I,I,

m"8

1 i

.5

.8

1.25

2.

RMS %
Error

Life Prediction Rati D Summary


0.

Figure 5.3.3.1 (Concluded)


5-27

.5

.8

1.25

2.

^ iNioo i
Condition/Ht:
Form:
Specimen Type: CT
Orientation:
Stress Ratio: 0.5
Frequency: 0.2 Hz

Yield Strength: 169.1 ksi


Ult. Strength: 236.5 ksi
Specimen Thk: 0.401 - 0.5 in.
Specimen Width:
Ref: PW006
(1 of 2)

AK (MPaVin)
4

10

I M'l'l

40

100

' I M'l'l

Environment: Lab Air; 800T

="]

(2 of 2)

AK (MPaVin)
- I

10

i I >|TI

40

100

' I M'l'l

Environment: Lab Air; 1350T 10

1
10

10

-=

10
10

10

_0J

2
io' ^

10

Z 10

10

io" ^

6^10-4

o 10
10

10

10

-3 I

T3

10

10

10

10

10

10

10

10

' i iiHI
40
100

'im

10

I , I,I,I,

I , I,I,I,

40

da/dN (10"6in/cycle)

AK (KsiVin)

.5

.8

1.25

14.6
14.7
18.5
23.7
43.0
57.7
87.0
102.

7.98 (min)
8.
9.
10.
13.
16.
20.
22.70 (max)

Life Prediction Ratio Summary

0.

100

da/dN (10"6in/cycle)

AK (KsiVin)

4.32
5.39
10.8
19.8
22.9

14.67 (min)
16.
20.
25.
27.30 (max)

10

AK (KsiVin)

AK (KsiVin)

2.50

D
X!

10

10

RMS %
Error

RMS %
Error
2.79

2.

Figure 5.4.3.1.1
5-28

Life Prediction Ratio Summary


.5

.8

1.25

IN100
Condition/Ht:
Form:
Specimen Type: CT
Orientation: CR
Frequency: 0.3 Hz
Environment: LAB AIR;1200F

AK (MPaVin)
4
10
40
100

-lI
= i ' i M'l'ir

Yield Strength: 169.1 ksi


Ult. Strength: 236.5 ksi
Specimen Thk: 0.5 in.
Specimen Width:
Ref: PW006
(1 Of 1)

4
prii i

I l I MM

AK (MPaVin)
10
40
100
i |i|i
I ' I Tl'l

10

- Stress Ratio: 0.05

10
10

10

10

10
10

10

_05

io" o

u
u 10

u
U 10

-3 EI

-3 |

10

10

E
10

10
10
"O

_s

10

10

10

10

10

10

10

10
'

10

i i 11 n

10

10

i i i tu

40

'

I I 11II

100

da/dN (10"6in/cycle)

AK (KsiVin)

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

27.2
29.2
54.2
72.8
91.2

19.64 (min)
20.
25.
30.
35.
40.
50.
50.85 (max)

RMS %
Error

10

AK (KsiVin)

AK (KsiVin)

5.90

_^"o
10

118.
244.
263.

Life Prediction Ratio Summary

RMS %

Life Prediction Ratio Summary

Error
i

.5

r-

.8

1.25

2.

Figure 5.4.3.1.2
5-29

0.

.5

.8

1.25

2.

I IN100 I
Condition/Ht:
Form:
Specimen Type: CT
Orientation: CR
Frequency: 0.3 Hz
Environment: LAB AIR;1200F

Yield Strength: 169.1 ksi


Ult. Strength: 236.5 ksi
Specimen Thk: 0.826 in.
Specimen Width:
Ref: PW006
(1 of 1)

AK (MPcVin)
4

10

- I I I 'I'l'l

40

AK (MPaVin)
4

100
1

I ' I 'I'l'l

10

- I ' I 'I'l'l

40

100

I ' I 'I'l'l

-= 10

- Stress Ratio: 0.05

10

10"2

10

-1

10

:
10"3

10
10

^
o

fri o"+
c
_

10

z. 10

/
&

o
6"10-4

io"2^
o
\
-3|

10 Ji_

-z.

zio"5

_A"o
10 a

\
a
^

10

10

>

-6

10

-5

10

10

10"7

10

-6

10

10
10

-1

- i ,

I,I,I,
4

1 , M.I.

10

40

la"8

- 1 , 1,1,1,
4

100

da/dN (10"6in/cycle)

Life Prediction Ratio Summary


i

0.

100

da/dN (I0"6in/cycle)

AK (KsiVin)

7.37
8.70
20.4

15.48 (min)
16.
19.71 (max)

RMS %
Error
3.41

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

1 , 1,1,1,

10

.5

.8

RMS %
Error

Life Prediction Ratio Summary

0.

1.25

Figure 5.4.3.1.3
5-30

.5

.8

1.25

IN100
Condition/Ht:
Form:
Specimen Type: CT
Orientation: CR
Frequency: 20 Hz
Environment: LAB AIR;800F

Yield Strength: 169.1 ksi


Ult. Strength: 236.5 ksi
Specimen Thk: 0.5 in.
Specimen Width:
Ref: PW006
(1 of 1)

AK (MPcVin)
4

10

40

= I ' I Tl'l

AK (MPaVin)
4

100

I ' I Tl'l

10

1 i 1 i nn

j.

40

100

' I 'I'l'l="

Stress Ratio: 0.1


-2

10

o
o 10

!^

10
-3

-2

io

Z 10
"O

JF

iw

_B
10

10

^io~2

o
10

E
10

-iTJ

10

-=Jio >

X>

10

10

10

10

" I , I.U.
4

10

i , I, I,i,

10

40

IiL

10
4

100

da/dN (10'6in/cycle)

AK (KsiVin)

'

10

1111 ii

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.915
1.02
2.01
4.57
8.08
13.7
15.3

12.40 (min)
13.
16.
20.
25.
30.
30.78 (max)

Life Prediction Ratio Summary

RMS %
Error

Life Prediction Ratio Summary


1

0.

U
40

AK (KsiVin)

AK (KsiVin)

RMS %
Error
9.45

-5

10
10

6-10-4

10

10

10

10
10

10

.5

.8

0.

lT25~
Figure 5.4.3.1.4
5-31

.5

.8

1.25

\ IN100 I
Condition/Ht:
Form:
Specimen Type: CT
Orientation: C-R
Frequency: 20 Hz
Environment: LAB AIR;1200F

Yield Strength: 169.1 ksi


Ult. Strength: 236.5 ksi
Specimen Thk: 0.108 in.
Specimen Width:
Ref: PW006
(1 of 1)

AK (MPcVin)
4

- I

10

40

1 I 'I'l'l

AK (MPaVin)
4

100

' 1 'I'l'l

Stress Ratio: 0.1

- I

10

' I 'I'l'l

40

100

' I 'I'l'l

10

-= 10
-2

10

10

10

10

10

10

0)

io" "

o
O-10-*

o
10
c

-3 r

10

Z. 10

10"

-=
"O

_B
10

.-6.

^-s

t"

'\
U
T3

10

10

10

10

10

-= 10

10

10

I
z

Z 10

*
10 >
-

"o

<p

2
10"

~~

"

I , LI,I,

I , I,I,I,

40

10

10

" I , I,I,I,
4

100

da/dN (10"6in/cycie)

Life Prediction Ratio Summary


i

0.

100

da/dN (10"6in/cycle)

AK (KsiVin)

10.0
10.6
15.5
15.9

24.21 (min)
25.
30.
30.86 (max)

RMS %
Error
8.06

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , I,I,I,

10

.5

.8

RMS %
Error

Life Prediction Ratio Summary

1.25

0.

2.

Figure 5.4.3.1.5
5-32

.5

.8

1.25

IN100
Condition/Ht:
Form:
Specimen Type: CT
Orientation: CR
Frequency: 0. Hz
Environment: LAB AIR;1100F

10

40

-Ml 'I'l'l

10

_a;
o
o 10
c

I ' I M'l'l

Z 10
T3

10

10

10

rJh

&8P

jn

cm

40

10

10
u

o
o 10

>

10

10

T3

10
10
10

10
4

100

10

40

100

AK (KsiVin)

da/dN (10"6in/cycle)

da/dN (10"6in/cycle)

AK (KsiVin)

15.9
20.4
41.9
73.4
107.
143.
183.
283.
429.

14.98 (min)
16.
20.
25.
30.
35.
40.
50.
60.
70.
72.77 (max)

RMS %
Error
21.34

10

10

AK (KsiVin)
AK (KsiVin)

10

10

100

' I 'I'l'l

10

10

I , Ml,I,

40

10"

10"2

-Jio

I , Ml,I,

10

' I 'I'l'l

10

10

dgP

"

- I

JL

10

EZ

AK (MPaVin)
4

100

Stress Ratio: 0.3

10

Yield Strength: 169.1 ksi


Ult. Strength: 236.5 ksi
Specimen Thk: 0.251 in.
Specimen Width:
Ref: PW006
(1 of 1)

AK (MPaVin)

650.
731.

Life Prediction Ratio Summary


i

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary

i-'

2.

0.

Figure 5.4.3.1.6
5-33

.5

.8

1.25

2.

^ IN100
Condition/Ht:
Form:
Specimen Type: CT
Orientation: CR
Stress Ratio: 0.1
Frequency:

Yield Strength: 169.1 ksi


Ult. Strength: 236.5 ksi
Specimen Thk: 0.246 - 0.461 in.
Specimen Width:
Ref: PW006

AK (MPaVin)
1

10

40

3)

100

- I
Environment: Lab Air; 800T

(2 of 3)

AK (MPaVin)

10

10

I I 'I'l'l

40

100

' I 'I'l'l

- Environment: Lab Air; 1200T


10

10

10

10

10

10
ju
o

6^10-4

-3 p
10 E

Z10

_
f

10"

-Jio>

10

10~

10

"o _e
10

"*-*
-2L

\'\
"

-o

""

10

10

10

10

10

10
10

-1

- I , I,I,I,
4

I , I,I,I.

10

40

10

- i , i,i,i,
4

100

da/dN (10"6in/cycle)

Life Prediction Ratio Summary


i

0.

40

100

da/dN (10'6in/cycle)

AK (KsiVin)

17.2
21.0
18.0

25.35 (min)
30.
30.46 (max)

RMS %
Error
17.50

i I i 11 li

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

.5

.8

RMS %
Error

Life Prediction Ratio Summary


i

0.

1.25

Figure 5.4.3.1.7
5-34

.5

.8

1.25

i-

2.

Condition/Ht:
Form:
Specimen Type: CT
Orientation: CR
Stress Ratio: 0.1
Frequency:

(3 of 3)

10

40

p.

AK (MPaVin)
1

100

Environment: Lab Air; 1350T 10

- I

la"2

10(1J 11

Yield Strength: 169.1 ksi


Ult. Strength: 236.5 ksi
Specimen Thk: 0.246 - 0.461 in.
Specimen Width:
Ref: PW006

AK (MPaVin)
1

IM

10

' I ' I'l'l

40

100

' I ' I'l'l

-1

10

io"2

-1

-1

10

10

io-3

jjffr

<D

o
c^10-+

Mr

B^

'

io"3

0)

io"

io~

<D

o
\

o
o^10-4

_3

10

0>

10

sE

"^

^s
5

2 10"

\
o
" -6

10

2 10"
"a
\
o
"^-6

>
XI

10

>
X>'

10

10

-5

-5

10

10

io-7

io'7

-6

-6

10
"

m-8

m"8 "

I , LM,

, I ,l,l,

10

10

40

U)0

1 , I.I.I;
4

6
da/dN (10 ~ in/cycle)

14.82 (min)
16.
20.
25.
30.
35.
40.
42.68 (max)

RMS %
Error
11.70

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

60 0
69 9
117.
217.
378.
623.
977.
1221.

Life Prediction Rati(3 Summary


0.

, I , l,l,

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

.5

1-

.8

RMS %
Error

Life Prediction Ratio Summary

1.25

0.

2.

Figure 5.4.3.1.7 (Concluded)


5-35

.5

.8

1.25

2.

-I IN100
Condition/Ht:
Form:
Specimen Type: CT
Orientation: CR
Stress Ratio: 0.1
Frequency: 0.2 Hz

Yield Strength: 169.1 ksi


Ult. Strength: 236.5 ksi
Specimen Thk: 0.5 in.
Specimen Width:
Ref: PW006
(1 of 2)

AK (MPaVin) .
1

- I

10

' I 'I'l'l

40

_L

' I 'I'l'l

Environment: Lab Air; 800T


-2

10

10

-o

- Environment: Lab Air; 1100T

z: 10

10

40
100
ni i i MM

z. 10

_Q3

o 10

4
10
{=Ii I i 1111

100

(2 of 2)

AK (MPaVin)

-3 |

raff
w
m

_R r10

10

-5

10

-7

10

10

-6

10

, I,I,I,
4

, I,I,I,

10

40

100

AK (KsiVin)
da/dN (10_6in/cycle)

AK (KsiVin)

RMS %
Error
22.81

.5

.8

1.25

100

12.0
17.0
31.7
54.1
77.7
99.7
123.
227.

14.26 (min)
16.
20.
25.
30.
35.
40.
50.
52.90 (max)

Life Prediction Ratio Summary


i

40

da/dN (10"6in/cycie)

AK (KsiVin)

3.24
4.71
6.30

16.43 (min)
20.
21.80 (max)

10

AK (KsiVin)

RMS %
Error
9.91

Figure 5.4.3.1.8
5-36

293.

Life Prediction Ratio Summary


i

0.

.5 .8

1.25

IN100
Condition/Ht:
Form:
Specimen Type: CT
Orientation: CR
Stress Ratio: 0.1
Frequency: 0.2 Hz

Yield Strength: 169.1 ksi


Ult. Strength: 236.5 ksi
Specimen Thk: 0.25 in.
Specimen Width:
Ref: PW006
(1 of 1)

AK (MPaVin)
4

- I

10

I I 'I'l'l

40

AK (MPaVin)
4

100

' I 'I'l'l

__i

10

| i ,|

40
100
I I ' I'l'l

FT

10

Environment: Lab Air; 1150T


10

10

10

10

io-3

10

io~2

-jio"2

O 10
c

J
10" E

_c

-z. 10
o

10

-3 I

_
10

10

-5
-

_*.Xf

10

X3

XI

10

10

__

10

10

10

10

10

- I , Ml
4

10

10

I , I,I,I,

10

40

10

da/dN (10"6in/cycle)

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

13.7
22.2
53.8

17.57 (min)
20.
23.45 (max)

RMS %
Error
10.89

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i i 11in

i i 11in

100

Life Prediction Ratio Summary


.5

.8

RMS %
Error

Life Prediction Ratio Summary


i

0.

1.25

Figure 5.4.3.1.9
5-37

ri

.5

.8

1.25

2.

-j IN100 I
Condition/Ht:

Yield Strength:
Ult. Strength:
Specimen Thk: 0.5 in.
Specimen Width: 2.5 in.
Ref: PW003

Form:
Specimen Type: CT
Orientation: CR
Stress Ratio: 0.1
Frequency: 30 Hz
(1 of 2)

AK (MPaVin)
4

=-l-"l I

10

40

Tlll

-2

10

I I ll>lll

"o

10

Environment: Lab Air; 500T

10

10
10

io"

o 10

-3 pr
10

10

.-5

10

J>

Jio >

f
f

-O

_A ~

10

1 , 1,1,1,
40

10
10
10

10

LL

100

.5

.8

1.25

I I I III

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.871
1.30
3.12
6.47
7.31

14.58 (min)
16.
20.
25.
26.09 (max)

0.130
0.507
1.43
3.67
5.88

Life Prediction Ratio Summary


0.

10

AK (KsiVin)

da/dN (10-6in/cycle)

14.09 (min)
16.
20.
25.
29.38 (max)

i I i I Hi

10

AK (KsiVin)
AK (KsiVin)

10

10

10

-3

, I,I,I,

T3

-5

ID

X3

RMS %
Error
20.62

10

' I M'l'l

40
100
' i i inn

_c

10 =

10

10
-

10

10

6^10-4 =
\
c
_

Z10-5

-1

10

100

Environment: Lab Air; 300F

(2 of 2)

AK (MPaVin)

2.

RMS %
Error
9.28

Figure 5.4.3.1.10
5-38

Life Prediction Ratio Summary


1

.5

.8

1.25

IN100
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CT
Orientation:
Frequency: 0.2 Hz
Environment: LAB AIR;1200F

10

Yield Strength: 169.1 ksi


Ult. Strength: 236.5 ksi
Specimen Thk: 0.252 - 0.302 in.
Specimen Width: 2.503 - 2.504 in
Ref: PW002
(1 of 2)

AK (MPaVin)
40

(2 of 2)

AK (MPaVin)
1

100

10

40

100

b I ' I 'I'l'lI ' I 'I'l'l


10

Stress Ratio: 0.1


10

10

Stress Ratio: 0.8


10

-1
10

10

10

10

_Q3

^jio~2

io"

o
o 10

10

o
_
o"l0-4

io- E

10

z: 10

"o

_c
10

>

^10
"o

,
10

-5
10

10

-7
10

10

10

10
.-8

10

i , i,i,i,

i , i, i. t.

40

10

10

100

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

50.
60.
67.89 (max)

5.85

0.

.5

.8

3.00
3.04
3.91
5.68
8.18
11.0
23.3
29.9

5.60 (min)
6.
7.
8.
9.
10.
13.
13.74 (max)

Life Prediction Ratio Summary

da/dN (10"in/cycle)

AK (KsiVin)

552.
624.
968.
1434.
1957.
2985.
5080.
7741.

23.52 (min)
25.
30.
35.
40.

I I I I III
40
100

I I I I III
4
10

AK (KsiVin)

RMS SB
Error

>
T3

1.25

2.

RMS %
Error
8.29

Figure 5.4.3.1.11
5-39

Life Prediction Ratio Summary

0.

.5

.8

1.25

2.

I IN100 I
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CT
Orientation: CR
Frequency: 20 Hz
Environment: LAB AIR;1200F

Yield Strength: 169.1 ksi


Ult. Strength: 236.5 ksi
Specimen Thk: 0.249 in.
Specimen Width: 2.501 in.
Ref: PW002
(1 of 1)

AK (MPaVin)
1

10

40

AK (MPaVin)
4

100

10

40

Stress Ratio: 0.05

100

-ii I i lim

C=-\I I I Mil

=n
10

-=
-2

10

10

10

10

-3

-3

10

10

o
6-10-4

u 10
c
Z10

10

/
/

__

Jio
>

10

_^_"o

-6
10
10

10

10

o
"

10

10

10

-3 I

10

3
10" E

- i ,

i ,

I,I,I,
4

10

10

10

I,I,I,
40

10

100

da/dN (10"*in/cycle)

Life Prediction Ratio Summary

0.

100

da/dN (10"6in/cycle)

AK (KsiVin)

4.32
4.75
7.10
12.6
20.9
30.8
38.1

14.03 (min)
16.
20.
25.
30.
35.
38.78 (max)

RMS %
Error
12.63

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

' i i 11 n

' i i i in
4
10

.5

.8

1.25

2.

RMS %
' Error.

Life Prediction Ratio Summary


i

0.

Figure 5.4.3.1.12
5-40

.5

.8

1.25

2.

IN100
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CT
Orientation: C-R
Frequency: 20 Hz
Environment: LAB AIR;1200F

Yield Strength: 169.1 ksi


Ult. Strength: 236.5 ksi
Specimen Thk: 0.206 - 0.442 in.
Specimen Width: 2.494 - 2.508 in
Ref: PW002
(1 of 2)

AK (MPaVin)
1

- I

10

40

' I M'l'l

100

' I 'I'l'l

- I

="

10

40

i I M'l'l

100
a

' I M'l'l

Stress Ratio: 0.8

10

Stress Ratio: 0.1

(2 of 2)

AK (MPaVin)

-2

-2

10

10

10

10

10

10

10"

-^io~
o
\

o
o^10-+

10
13

10

-= 10"

E
Z 10

10
O

o
u 10

"O

tZ

"O

-6
10

_B ~

10

I
z:

m~ ^
u

10

<D

XJ

10

10

10
-6

10

10
10

I , Mil,

I , 1,1,1.

40

10

10

100

da/dN (10"6in/cycle)

RMS %
Error
17.40

.5

.8

100

0.346

4.39 (min)
5.
6.
7.
8.
9.
10.
11.78 (max)

Life Prediction Ratio Summary


no
0.

40

da/dN (10"6 in/cycle)

AK (KsiVin)

3.94
4.92
8.16
15.2
25.3
36.6
46.6
49.0

13.55 (min)
16.
20.
25.
30.
35.
40.
41.45 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , I,I,I,

~ I , LI,I,

1.25

RMS %
Error
6.08

Figure 5.4.3.1.13
5-41

0.613
0.990

1.29
1.63
2.14
2.81

4.09

Life Prediction Ratio Summary

0.

.5

.8

1.25

2.

1 IN100 I
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CT
Orientation: CR
Frequency: 0.2 Hz
Environment: LAB AIR;1200F
(1 of 2)

AK (MPaVin)
4

= I

10

40
100
i Ml'l'l

' I 'I'M

Yield Strength: 169.1 ksi


Ult. Strength: 236.5 ksi
Specimen Thk: 0.5 - 0.503 in.
Specimen Width: 2.496 - 2.505 in
Ref: PW002
(2 of 2)

AK (MPaVin)
4

10

40

I ' I M'l'l

I ' I M'l'l

=q

100
10

Stress Ratio: 0.8

Stress Ratio: 0.5


10

10
10

io"2

o
4

0-10-

10
-Z. 10
a

"I

\
o
~0

-4^?
o

-6

10

10

10
10

10

40

100

RMS %
Error
5.87

Life Prediction Ratio Summary


no
0.

.8

15.4
20.4
30.3
57.3
80.1

9.28 (min)
10.
13.
16.
18.16 (max)

2.69
3.22
4.41
12.1
23.2
43.0
62.8

.5

100

da/dN (I0"6in/cycle)

AK (KsiVin)

da/dN (10-6in/cycle)

8.06 (min)
9.
10.
13.
16.
20.
22.91 (max)

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

UJi

I [Mill.
4
10

10

1.25

RMS %
Error
4.32

Figure 5.4.3.1.14
5-42

Life Prediction Ratio Summary


a
i

0.

.5

.8

1.25

2.

IN100
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CT
Orientation: CR
Stress Ratio: 0.1
Frequency:

Yield Strength: 169.1 ksi


Ult. Strength: 236.5 ksi
Specimen Thk: 0.25 - 0.856 in.
Specimen Width: 2.436 - 2.51 in.
Ref: PW002
(1 of 2)

AK (MPaVin)
1

10

40

100

- I
Environment: Lab Air;1200T

10

10

*
_

10"

-3 |

10

Z 10
a

-a

_fi

__

-o

10

tz
_R

10

10

L"0

-5

-r: 10

-= 10

10

10

10

.-8

-=:

"""

J
10 >

10

o
6-10-4
\
c
_

ZIG"5

10

100

' | MM'I

10

"U

40

10

\
o

10

i I >|i|i|

Environment: Lab Air; 1350T 10

10

-2

10

6^10_c

(2 of 2)

AK (MPaVin)

I , I,I,I,

- i , i,i,i,
4

10

10

10

40

10

RMS %
Error
47.00

40

100

da/dN (10-6in/cycle)

AK (KsiVin)

da/dN (1Cr6in/cycle)

105.
107.
293.
776.
871.

12.93 (min)
13.
16.
20.
21.29 (max)

85.6
84.7
106.
203.
408.
755.
1237.
2413.
4198.
6600.

15.61 (min)
16.
20.
25.
30.
35.
40.
50.
60.
67.35 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , LLL

~ I . I , l,l.

100

Life Prediction Ratio Summary


A x
+ ' o
I

0.

.5

.8

1.25

2.

RMS %
Error
10.90

Figure 5.4.3.1.15
5-43

Life Prediction Ratio Summary


a
i

0.

.5

.8

1.25

I IN100 I
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CT
Orientation: CR
Stress Ratio: 0.1
Frequency: 0. Hz

Yield Strength: 169.1 ksi


Ult. Strength: 236.5 ksi
Specimen Thk: 0.25 - 0.469 in.
Specimen Width: 2.437 - 2.511 in
Ref: PW006;PW002
(1 of 2)

AK (MPaVin)
4
10
I I ' I 'Ml

(2 of 2)

AK (MPaVin)
4

40
100
Ti I i I Mil

10

- I ' I 'I'l'l

-Environment: Lab Air; 1200T 10


-2

10

10

40

'

u 10
c
Z 10
a
10

-1

Environment: Lab Air; 1350F 10

10

j
V
io"2^

-al
_

-=

T3

100

i'l'l

J
f

10

10

10
4

10

40

"

ZL

, I,I,I,
4

100

da/dN (10'6in/cycle)

25.
30.
35.
40.
50.
60.
70.
80.
90.
91.39 (max)

RMS *
Error

9.35

HA
i

.5

.8

40

100

da/dN (10"6in/cycle)
281.
322.
452.

27.86 (min)
30.
35.
40.
50.
60.
65.70 (max)

Life Prediction Ratio Summary


0.

AK (KsiVin)

22.7
23.4
34.7
65.7
120.
199.
295.
497.
700.
927.
1207.
1569.
1628.

15.43 (min)
16.
20.

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , M,!<

-6

10

1.25

RMS %
Error
6.80

Figure 5.4.3.1.16
5-44

630.
1117.
1699.
2019.

Life Prediction Ratio Summary


r-

0.

.8

1.25

This page intentionally left blank

5-45

1 IN100 I
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CT
Orientation: CR
Stress Ratio: 0.1
Frequency: 0.2 Hz

Yield Strength: 169.1 ksi


Uit. Strength: 236.5 ksi
Specimen Thk: 0.25 - 0.87 in.
Specimen Width: 2.493 - 2.511 in
Ref: PW002;PW006
(1 of 4)

AK (MPaVin)
4

10

- I ' I Tl'l

40

100

I ' I Tl'l

4
10
I I I Mill

~~

-2

6^10c

_2

~~

10

o
o 10

-3|
10 E

10

t"

in '\
u

10

10
10

10
=

10

~ 10

- I , LI,I,
4

10

, I,I,I,

10

40

'

10

i i 11 n

100

da/dN (10"6in/cycle)

AK (KsiVin)

25.
30.
35.
40.
50.
57.86 (max)

.5

.8

100

7.25
16.9
35.3
61.9
89.9
120.
153.
239.
338.

13.17 (min)
16.
20.

Life Prediction Ratio Summary


0.

40

da/dN (10'6in/cycle)

AK (KsiVin)

9.13
11.9
17.6
24.6
33.2
45.8
65.2
72.1

14.22 (min)
16.
20.
25.
30.
35.
40.
41.33 (max)

10

AK (KsiVin)

AK (KsiVin)

RMS X
Error
2.53

-o

XJ

10

<0

_*
10

10

z 10~ I

10
-o

10

10~
c;
\

_
-5

10

10

100

10

40

i i i innni

Environment: Lab Air; 1200T -=i 10

Environment: Lab Air; 1000T


10

(2 of 4)

AK (MPaVin)

1.25

2.

RMS %
Error
10.05

Figure 5.4.3.1.17
5-46

Life Prediction Ratio Summary


0.

.5

.8

1.25

IN100
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CT
Orientation: C-R
Stress Ratio: 0.1
Frequency: 0.2 Hz

Yield Strength: 169.1 ksi


Ult. Strength: 236.5 ksi
Specimen Thk: 0.25 - 0.87 in.
Specimen Width: 2.493 - 2.511 in
Ref: PW002;PW006
(3 of 4)

AK (MPaVin)
4
10
crli i i i ill

(4 of 4)

AK (MPaVin)

40
100
1 I I I Mil

-1

4
10
I MUM

1I

40
100
I I IHM

Environment: Lab Air; 1350T

- Environment: Lab Air; 1300T 10

10

10
10
10

^io"2

o
^10"4

o
\

ho
10

\
O
"O

_*-o
10

o
X)

_K i
10
10
-7

10

10
' i i i in
4
10

10

' i i 11 n
40
100

da/dN (10"6in/cycle)

AK (KsiVin)

54.45 (max)

Life Prediction Ratio Summary

0.

.5

.8

40

100

. da/dN (10"6in/cycle)
17.7
24.3
50.8
99.7
157.
186.
355.
546.

14.68 (min)
16.
20.
25.
30.
35.
40.
41.46 (max)

110.
153.
197.
280.
313.

50.

RMS %
Error
4.18

AK (KsiVin)

39.0
70.7

20.20 (min)
25.
30.
35.
40.

10

AK (KsiVin)

AK (KsiVin)

1.25

RMS %
Error
8.64

Life Prediction Ratio Summary


a
i

0.

Figure 5.4.3.1.17 (Concluded)


5-47

.5

.8

1.25

2.

\ IN100 I
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CCP (max load specified)
Orientation:
Stress Ratio: 1
Frequency: 0.2 Hz
(1 of 2)

AK (MPaVin)
4

- I

10

' I M'l'l

40

Yield Strength: 169.1 ksi


Ult. Strength: 236.5 ksi
Specimen Thk: 0.298 - 0.299 in.
Specimen Width: 0.995 - 1 in.
Ref: PW002

100

_L

' I 'I'l'l

(2 of 2)

AK (MPaVin)
i

4
10
i i i|i|i|

40
100
i | i|TI

Environment: Lab Air; 800F

10

10

ID"3

10

_a;
o
o 10

o^10\
c
_

10

^E

a)

10"

10" N
-^
z

jjp

$r

Z10
T3

z: 10
p

10

10

10

/
10

10

10
10
.-8

10

i , i,i,i,

i , I,I,I,

40

10

10

m"

10
-=

~ I , I,I,I,
4

100

RMS %
Error

3.39

.5

.8

10

, I,I,I,
40

100

da/dN (10"6in/cycle)

AK (KsiVin)

37.8
38.5
62.4
91.0
132.
196.
253.

19.84 (min)
20.
25.
30.
35.
40.
42.98 (max)

1.06
1.96
3.97
10.3
16.6

Life Prediction Ratio Summary


0.

AK (KsiVin)

da/dN (10"6in/cycle)

13.48 (min)
16.
20.
25.
26.54 (max)

o
-o

10

AK (KsiVin)
AK (KsiVin)

-i

Environment: Lab Air; 1200T

1.25

RMS %
Error
4.70

Figure 5.4.3.1.18
5-48

Life Prediction Ratio Summary


0.

.5

.8

1.25

IN100
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CCP (max load specified)
Orientation:
Stress Ratio: 0.5
Frequency: 0.2 Hz
(1 of 2)

AK (MPaVin)
4

- I

10

40

' I 'I'l'l

Yield Strength: 169.1 ksi


UK. Strength: 236.5 ksi
Specimen Thk: 0.228 - 0.309 in.
Specimen Width: 0.988 - 1.038 in
Ref: PW002

100
a

' I 'I'l'l

-2

10

10
10

10

10

.2

io"2

J
f

z: 10

10

10

"o

XI

10

10
4

I , LI,I,

10

-= 10

40

31.05 (max)

-= 10

^
u
x>

10

- I , Ml,I,
4

I i M IJ,

10

40

100

.8

1.25

da/dN (10"6in/cycle)

AK (KsiVin)

12.2
21.5
41.1
73.7
128.
186.

13.75 (min)
16.
20.
25.
30.
33.24 (max)

Life Prediction Ratio Summary


1

-z.

1.13
1.75
4.11
7.40
15.4
44.4
58.2

.5

Jjr

AK (KsiVin)

25.
30.

10"
*
-

<m

100

12.10 (min)
13.
16.
20.

0.

<D

2 Tt
O

_e I
10

10

10

da/dN (10"6in/cycle)

AK (KsiVin)

-1

AK (KsiVin)

RMS %
Error
16.76

I ' I 'I'l'l

-J10>

- i , i,i,i,

100

Environment: Lab Air; 1200T =.

2 10

10

10

40

oMo"4

fri o"

10

-Ml
'I'l'l

10

Environment: Lab Air; 800T

(2 of 2)

AK (MPaVin)

2.

RMS %
Error
9.05

Figure 5.4.3.1.19
5-49

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

1 IN100 I

Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CCP (max load specified)
Orientation: C-R
Frequency: 0.2 Hz
Environment: LAB AIR;1200F
(1 of 1)

AK (MPaVin)
4

10

40

z I M 'I'l'l

Yield Strength: 169.1 ksi


Ult. Strength: 236.5 ksi
Specimen Thk: 0.296 in.
Specimen Width: 0.986 in.
Ref: PW002

AK (MPaVin)
4
10
I I I I'l'l

100
1

I ' I 'I'l'l

Stress Ratio: 0.1

10
10

"

10

10

10

10
io"
o

o
\

O
4

o^10-

5^10-

-3 I

10

^~

10

10

_
R ~
-6

10

10

10

10

10

10

" I , Li,l,
4

10

10

I , l,l,l,

10

40

10

100

Life Prediction Ratio Summary


0.

I I III
40
100

da/dN (10~6 in/cycle)

AK (KsiVin)

6.62
6.72
12.0
28.4
64.0
95.9
101.

12.89 (min)
13.
16.
20.
25.
30.
31.93 (max)

10

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

I I 11 ll

AK (KsiVin)

RMS %
Error
11.71

10

Z 10

10

-no"2

-o

100

' I 'I'l'i="

-=

10

40

.5

.8

1.25

2.

RMS %
Error

Life Prediction Ratio Summary


,

0.

Figure 5.4.3.1.20
5-50

.5

.8

1.25

2.

IN100
Condition/Ht: PRESTRAIN
Form: 1.6 in. Forging
Specimen Type: CCP (max load specified)
Orientation:
Frequency: 0.2 Hz
Environment: LAB AIR;1200F
(1

10

40

I 'I'I'I

of 1>

AK (MPaVin)
4

100

' I 'I'I'I

Stress Ratio: 0.1

10

40

100

I III

Yield Strength: 169.1 ksi


Ult. Strength: 236.5 ksi
Specimen Thk: 0.288 in.
Specimen Width: 0.722 in.
Ref: PW002

I III \-

AK (MPaVin)

10
-2

10

10

-3

10

10

0)

o
^10"4

-5

10

10

10

o
x>

10

TJ

10

o
6^10-4
c
_

10

X>

10

10

10

10
10

10

10

10
i

I i 1,1

i i i i n

10

10

40

"

100

I , I . I.I.

I , I,I,I,

40

da/dN (10'6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


i

100

2.52
4.06
15.8
34.0

11.89 (min)
13.
16.
19.36 (max)

0.

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
30.81

10

10

10

10

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary

.5

2.

Figure 5.4.3.1.21
5-51

.8

1.25

H IN100 P/M-G I

1600F 0.67HR AC
Yield Strength: 158.2 ks I
Ult. Strength: 176.9 ksi
Specimen Thk: 0.5 in.
Specimen Width: 2.5 in.
Ref: PW004

Condition/Ht: 2050F 2HRS OQ


Form: Disk
Specimen Type: WOL
Orientation: C-R
Stress Ratio: 0.05
Environment: LAB AIR;1200F

AK (MPaVin)
4

- I

10

' I 'I'l'l

40

' I TW>
<
*rtt\

lO"2

~ 10

___

40

100

10

10"2
-1

-1

10

10

10

-X

io"

io"2

0>

o 10

Z10-5
\

10

E
^-^

o
u 10
\

JP
JBi
Jj

zio"
>

JF

^-s

10

10

\
o

-s

-5

10

10

io"7

-6

-6

10

10
m"

I , !,U

I , I. I,I,

10

40

in"8

100

RMS %
Error
32.41

.5

.8

, 40

100

6
da/dN (10 " in/cycle)

AK (KsiVin)
13.36 (min)
16.
20.
25.
30.
35.
40.
43.75 (max)

503.
518.
751.
1176.
1875.
4591.
10161.
20114.
35904.
58501.
80363.

Life Prediction Ratio Summary


0.

10

AK (KsiVin)

da/dN (10"6in/cycle)

24.49 (min)
25.
30.
35.
40.
50.
60.
70.
80.
90.
97.60 (max)

I , 1.1,1,

" I , l.l.l,
1

AK (KsiVin)
AK (KsiVin)

o
\
-3|
10 E
^~^

10

io"7

jibo

10

- I ' I ' I'l'l


I ' 1 ' I'l'l
Frequency: 0.01 Hz

~"

100

Frequency: 0. Hz

(2 of 4)

AK (MPaVin)

4)

1.25

2.

RMS %
Error
22.51

Figure 5.5.3.1
5-52

4.70
10.7
25.9
53.8
88.7
127.
165.
194.

Life Prediction Ratio Summary


0.

.5

.8

1.25

2.

IN100 P/M-G

(3 of 4)

AK (MPaVin)
1

10

= I ' I 'I'l'l

40
-1

1600F 0.67HR AC
Yield Strength: 158.2 ksi
Ult. Strength: 176.9 ksi
Specimen Thk: 0.5 in.
Specimen Width: 2.5 in.
Ref: PW004

Condition/Ht: 2050F 2HRS OQ


Form: Disk
Specimen Type: WOL
Orientation: C-R
Stress Ratio: 0.05
Environment: LAB AIR;1200F

4
10
i I ' I'l'l

100

I I I Mil

(4 of 4)

AK (MPaVin)

40
100
1i I i I'l'l

10

Frequency: 0.33 Hz
-2

10

-1

10
10

10
10

-5

10

10
-a

.-6

10

10
10
10
10
4

10

40

100

da/dN (10~6in/cycle)

AK (KsiVin)

35.
40.
46.90 (max)

RMS %
Error

19.36

1~'

0.

.8

100

1.25

4.26
4.29
6.15
10.7
17.5
25.9
34.5
43.3

15.92 (min)
16.
20.
25.
30.
35.
40.
46.70 (max)

Life Prediction Ratio Summary


.5

40

da/dN (10"6in/cycle)

AK (KsiVin)

2.78
7.49
18.5
34.1
49.2
64.3
81.4
112.

13.44 (min)
16.
20.
25.
30.

10

AK (KsiVin)

AK (KsiVin)

2.

RMS %
Error
25.22

Life Prediction Ratio Summary


i

0.

Figure 5.5.3.1 (Concluded)


5-53

.5

.8

1.25

2.

i INCOLOY 901 I
Condition/Ht:
Form:
Specimen Type: CT
Orientation: CR
Frequency: 20 Hz
Environment: LAB AIR;900F

Yield Strength:
Ult. Strength:
Specimen Thk: 0.5 in.
Specimen Width: 2.5 in.
Ref: PW003
(1 of 1)

AK (MPcVin)
4

_ I

10

1 I in*!

40

AK (MPaVin)
4
10
crii i i Mil

100

i 1 >lllll

J.

40
100
-\l I I i mi
10

-= 10

Stress Ratio: 0.05

-2

10

10

10

10

10

10
-2

io

o
+

l 0"

\
c

^9

"""**
_

""~
TO

10
""""

.2

o
6^10-4

-3 |

10

Z 10

10

10" E

x>
\
o

xi

"

10

10

10

10

10
10

10

10

10
10

-el-

- 1 , 1,1,1,
4

-8

i,\,\,\,

10

40

10

'

I I IIII

100

da/dN (10"6in/cycle)

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


I

100

0.779
1.00
2.20
4.87
9.23
15.6
24.3
48.7
68.7

14.89 (min)
16.
20.
25.
30.
35.
40.
50.
56.30 (max)

RMS %
Error
24.06

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

II

10

.5

.8

RMS %
Error

Life Prediction Ratio Summary


i

0.

1.25

Figure 5.6.3.1
5-54

.5

.8

1.25

This page intentionally left blank

5-55

1 INCONEL 600 I
Condition/Ht: 1585F .75HR AC
Form: 1 in. Plate
Specimen Type: CT
Orientation:
Frequency: 6.7 Hz
Environment: LAB AIR;1000F
(1 of 2)

AK (MPaVin)
4

- I

10

I I ll'l>l

40

Yield Strength: 35 ksi


Ult. Strength: 94.3 ksi
Specimen Thk: 0.41 - 0.413 in.
Specimen Width: 2.002 - 2.004 in
Ref: HD003

100

' l'l'l'l

Stress Ratio: 0.5

(2 of 2)

AK (MPaVin)
10

40

100

10

-2

10

10

Stress Ratio: 0.66

10

10

-2

10
:
10

10

10

o
frl 0"+

Z10"5
-o
tz
Q

o
\

o
:
6-10-4

10

10

"o

XI

10

_K I
10

10

-7

10

10

" 1 , 1,1,1,
4

40

10

~ I , I,hi,
4

100

da/dN (10"6in/cycle)

RMS %
Error
2.32

.5

.8

100

0.215
0.251
0.368
0.521
0.674
0.955

6.43 (min)
7.
8.
9.
10.
11.40 (max)

Life Prediction Ratio Summary


0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.688
0.861
1.73
3.53
4.03

9.14 (min)
10.
13.
16.
16.53 (max)

I , I,I,I,

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

o
x>

10

1 , 1,1,1,

10

10

10

10
-8

T3

10

1.25

RMS %
Error
1.47

Figure 5.7.3.1.1
5-56

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

INC0NEL 600
Condition/Ht: 1585F .75HR AC
Form: 1 in. Plate
Specimen Type: CT
Orientation:
Frequency: 6.7 Hz
Environment: LAB AIR;800F

Yield Strength: 35 ksi


Ult. Strength: 94.3 ksi
Specimen Thk: 0.413 in.
Specimen Width: 2.002 in.
Ref: HD003
(1 of 1)

AK (MPaVin)
4

10

' I M'l'l

.40
100
ni i i i Mil

AK (MPaVin)
4

=q

10

40
-I

F=~1i I MM'

100

I I Mill

10

10

Stress Ratio: 0.6

-2

-2

10

10

10

10
10

ID"3
2

-J10"

G-10-4

^io-+
10
Z 10
xs
x>

10

E
"o

_x"a
10
o

10

-5

10

10

-7

10

10

10

10
i

'

I Mill

10

I ' I ill

40

10

I i I I li

100

da/dN (10"6in/cycie)

AK (KsiVin)

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.172
0.176
0.250
0.379
0.547
0.818

6.90 (min)
7.
8.
9.
10.
12.06 (max)

Life Prediction Ratio Summary


0.

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
7.46

XI

_R -

10

.-8

10
x>

X>

_c
.-6
10

10

.5

.8

RMS ss
Error

Life Prediction Ratio Summary


i-'

0.

1.25

Figure 5.7.3.1.2
5-57

.5

.8

1.25

2.

^ INCONEL 600 I
Condition/Ht: 1585F .75HR AC
Form: 1 in. Plate
Specimen Type: CT
Orientation:
Stress Ratio: 0.05
Frequency: 0.7 Hz
(1 of 4)

AK (MPaVin)
4
10
(=Ii I i I'M

Yield Strength: 35 ksi


Ult. Strength: 94.3 ksi
Specimen Thk: 0.396 - 0.482 in.
Specimen Width: 1.997 - 2.005 in
Ref: HD003

40
100
-ii i i i UM

Environment: Lab Air; 600T

10

-Ml 'I'l'l
10

10

io"2^

10

-3 f

10

10
10

40

100

I ' I Tl'l

XI

10
-5

10

-3
10

o 10

\
c
_

Z. 10

-a _
10

M
&

10

10
10

i I i I M
4
10

i i i

40

.-8

10

HI

100

-^ 10

i , i,i,i,

I , I,l,l,

40

RMS 55
Error
14.42

.5

.8

100

da/dN (10"6in/cycle)

AK (KsiVin)

4.60
6.72
15.2
20.8

22.56 (min)
25.
30.
32.19 (max)

4.25
11.5
17.2

Life Prediction Ratio Summary

0.

10

AK (KsiVin)

da/dN (10~6in/cycle)

25.08 (min)
30.
31.85 (max)

= 10

AK (KsiVin)
AK (KsiVin)

10
-2T
10"
-3 I
10 E

Jio
>
z.

10

10

_L

Environment: Lab Air; 800T

10

10

J2

(2 of 4)

AK (MPaVin)

RMS %
Error
4.10

1.25

Figure 5.7.3.1.3
5-58

Life Prediction Ratio Summary


a

0.

.5

.8

1.25

INCONEL 600
Condition/Ht: 1585F .75HR AC
Form: 1 in. Plate
Specimen Type: CT
Orientation:
Stress Ratio: 0.05
Frequency: 0.7 Hz
(3 of 4)

AK (MPaVin)
4

10

40

Yield Strength: 35 ksi


Ult. Strength: 94.3 ksi
Specimen Thk: 0.396 - 0.482 in.
Specimen Width: 1.997 - 2.005 in
Ref: HD003

100

10

40

' I 'I'l'lI

100

' I 'I'l'l

10

Environment: Lab Air; 1200T


10

10

-3

10

10

10

10

.2?

^10"

Z 10

o
\

-3 |

10

-3 |

10

-Z. 10

/
/

T3

J2>

o
6-10-4

o
\

XI

= I

- I 1 I "I'l'l
1 ' 1 'I'l'l
-L
Environment: Lab Air; 1000T -= 10

\
c

(4 of 4)

AK (MPaVin)

-Jio->

_A"U

10

XI

-O

_B

10

10

10

10

10

10

10

" I , Mil,
4

10

10

1 , 1,1,1,

10

40

10

I I I 111

100

da/dN (10"6in/cycle)

RMS %
Error
8.71

RTVM-

.5

.8

4.53
7.58
16.7
21.2

14.24 (min)
16.
20.
23.73 (max)

Life Prediction Ratio Summary


0.

100

da/dN (10"6in/cycle)

AK (KsiVin)

4.34
5.04
11.0
22.0
28.2

18.57 (min)
20.
25.
30.
32.64 (max)

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I -1 I 11II

10

1.25

RMS %
Error
28.60

Life Prediction Ratio Summary


a o
i

0.

Figure 5.7.3.1.3 (Concluded)


5-59

.5

.8

1.25

2.

\ INCONEL 600 I
Condition/Ht: 1585F .75HR AC
Form: 1 in. Plate
Specimen Type: CT
Orientation:
Stress Ratio: 0.05
Frequency: 5 Hz
(1 Of 1)

AK (MPaVin)
4
I-

10

40
"II

' I ' Ml'

Yield Strength: 35 ksi


Ult. Strength: 94.3 ksi
Specimen Thk: 0.39 in.
Specimen Width: 2 in.
Ref: HD003

AK (MPaVin)
4

100
c=1i
E~r

I ' MI'I

Environment: Lab Air; R.T.

10

40

100

"1I I I I 'Ml

I i Ml'

10

10

10

10

10

10

10

10

-2
-M0'2

io~

l 0"+
10

o
\

o
6-10-4

-3 I

10

v
z.

-5

10

10
T3

iT>

10

10

10

10

10

10

10

10

10

10
i

' i iiHI
4
10

10

10

I i lili
40
100

'

da/dN (10"6in/cycle)

0.

100

da/dN (10'6in/cycle)

AK (KsiVin)

10.3
18.7
19.8

Life Prediction Ratio Summary


i

i i ii ii

40

2.73
5.03

25.33 (min)
30.
35.
40.
40.56 (max)

RMS %
Error
3.56

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'

I i I Hi

RMS %
Error

.5

.8

Life Prediction Ratio Summary


i-

.5

1.25
Figure 5.7.3.1.4
5-60

.8

1.25

2.

INCONEL 600
Condition/Ht: 1585F .75HR AC
Form: 1 in. Plate
Specimen Type: CT
Orientation:
Stress Ratio: 0.05
Frequency: 6.7 Hz
(1 of 2)

AK (MPaVin)
4
10
prIi i i i Hi

40
-1

Yield Strength: 35 ksi


Ult. Strength: 94.3 ksi
Specimen Thk: 0.412 - 0.414 in.
Specimen Width: 2.002 in.
Ref: HD003

100

I I I INI

- Environment: Lab Air; 800T

10

I I I IMI

(2 of 2)

AK (MPaVin)
40
1

100

| I |l|l|

Environment: Lab Air; 1000T 10

-2

10

10

10

10

10

10
10

o
o 10

10

-JicT E

10~2
o
6-10-4

10

10

^10

>
o

10
-a

10

10

10

10
10

10

10

10
i Mini
40
100

10
4

10

'

10

da/dN (10"6in/cycle)

.5

.8

1.25

1.55
3.85
11.8
22.9
23.9

16.50 (min)
20.
25.
30.
30.56 (max)

Life Prediction Ratio Summary


0.

Mini
40
100

da/dN (10"6in/cycle)

AK (KsiVin)

0.660
1.71
5.27
9.39

16.89 (min)
20.
25.
27.20 (max)

RMS %
Error
5.32

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i i 11 n

2.

RMS %
Error
3.90

Figure 5.7.3.1.5
5-61

Life Prediction Ratio Summary


a
.5

.8

1.25

2.

^ INCONEL 600 I
Condition/Ht: 1585F .75HR AC
Form: 1 in. Plate
Specimen Type: CT
Orientation:
Stress Ratio: 0.33
Frequency: 6.7 Hz

Yield Strength: 35 ksi


Ult. Strength: 94.3 ksi
Specimen Thk: 0.413 in.
Specimen Width: 2.002 - 2.003 in
Ref: HD003
(1 of 2)

AK (MPaVin)

(2 of 2)

AK (MPaVin)
4

4
10
40
100
1i I i I i|i|
I I I I MM
- Environment: Lab Air; 800F 10

10

40

100

1I I I 11111

' I M'l'l

Environment: Lab Air; 1000T 10


10

10

10

10
10

10

-lio"2^

frlO"4

6^10-

-3 |

10
10
10

10

XI

X>

"

X>

10

E^

-z.

10
10

o
x>

-sl-

10

10

10
-7

10

10

10

10
-8

10

'

10

10

I I I I III
40
100

I I III!

da/dN (10"6in/cycle)

RMS %
Error
4.09

0.989
1.34
2.75

6.69
9.16

22.90 (max)

0.

100

16.
20.

Life Prediction Ratio Summary


.8

40

11.70 (min)
13.

3.92
4.77

.5

i 11 it

da/dN (10"6in/cycle)

AK (KsiVin)

0.482
0.627
1.34

12.17 (min)
13.
16.
20.
20.75 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i i 1111

1.25

RMS %
Error
3.06

Figure 5.7.3.1.6
5-62

Life Prediction Ratio Summary


a
i

0.

.5

.8

1.25

2.

INCONEL 625

I
s
a

IP

mm

lillll
M*MMMMMHMMMMMMMMMMHNNtMMMlM

CO
10

c
H

II

GO

I
3
s
o

5-63

i INCONEL 625
Condition/Ht: MA
Form: 1 in. Plate
Specimen Type: CT
Orientation:
Stress Ratio: 0.05
Frequency: 0.7 Hz

Yield Strength: 65.9 ksi


Ult. Strength: 132.9 ksi
Specimen Thk: 0.299 - 0.445 in.
Specimen Width: 1.153 - 2.002 in
Ref: HD005
(1

AK (MPaVin)
4

= I

10

' I 'I'l'l

40

of 4)

4
10
I I I IHM

100

' I 'l'l'l

40

100

I I'l'l'1
Environment: Lab Air; 800F

-= 10

Environment: Lab Air; 600F

(2 of 4)

AK (MPaVin)

-2

10

10

10

10

10

10

_Q5

6-10-

i o"
c

10

10"

-J10
>

o
\

1
<
o
T3

_K
.-6
10

-z.

Z 10

10
-o

10"

10
10

10

10

10

10

10
10

i . 1.1,1,

I , i .i.i.
4

10

40

'

10

100

da/dN (10"6in/cycle)

25.
30.
35.
40.
46.44 (max)

RMS %
Error
25.35

.5

.8

4.04
5.70
11.7
23.7
43.2
69.1
92.1

16.88 (min)
20.
25.
30.
35.
40.
44.02 (max)

Life Prediction Ratio Summary


an
a
0.

da/dN (10'6in/cycle)

AK (KsiVin)

1.51
3.33
9.73
21.2
39.0
65.0
115.

17.31 (min)
20.

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I I I I III
40
100

l i li li

1.25

2.

RMS %
Error
22.59

Figure 5.8.3.1.1
5-64

Life Prediction Ratio Summary

o
-V

0.

.5

.8

1.25

NCONEL 625
Condition/Ht: MA
Form: 1 in. Plate
Specimen Type: CT
Orientation:
Stress Ratio: 0.05
Frequency: 0.7 Hz

Yield Strength: 65.9 ksi


Ult. Strength: 132.9 ksi
Specimen Thk: 0.299 - 0.445 in.
Specimen Width: 1.153 - 2.002 in
Ref: HD005
(3 of 4)

AK (MPaVin)
4

10

-I'M I'l'l
10

40

Environment: Lab Air; 1000F

10

-o

_K
.-6

10

10

' I 'I'l'l

40

100

' I 'I'l'l
10

Environment: Lab Air; 1200F


10

10

10

10

JE

-Jio'2

o
u 10

uf'I

10
10

-Jio
\
"~

-A~0

10

10

-5

10

10
10

10

10

10

XI

10

- I

io"

fri a"
c

1
_L

(4 of 4)

AK (MPaVin)

100
MINI

'

10

, I,I,I,
4

I , Mil,

10

40

10

I I I I 11

100

da/dN (10"6in/cycle)

RMS %
Error
11.99

CD

.5

.8

5.39
8.63
17.1
32.7
52.5
74.2
91.0

13.75 (min)
16.
20.
25.
30.
35.
38.90 (max)

Life Prediction Ratio Summary


0.

100

da/dN (10"6in/cycle)

AK (KsiVin)

5.62
5.92
9.27
17.0
30.4
51.6
82.9
111.

15.46 (min)
16.
20.
25.
30.
35.
40.
43.39 (max)

I 11 III

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

1.25

RMS %
Error
10.79

Life Prediction Ratio Summary


0.

Figure 5.8.3.1.1 (Concluded)


5-65

.5

.8

1.25

2.

^ INCONEL 625
Condition/Ht: MA
Form: 1 in. Plate
Specimen Type: CT
Orientation:
Stress Ratio: 0.05
Frequency: 10 Hz

Yield Strength: 65.9 ksi


Ult. Strength: 132.9 ksi
Specimen Thk: 0.295 in.
Specimen Width: 1.153 in.
Ref: HD005
(1 of 1)

AK (MPaVin)
4

10

40

-"I ' I M'l'l

AK (MPaVin)
4

100

' I M'l'l

10

40

TTTT

100

' I M'l'l

-= 10

Environment: Lab Air; R.T.

10

-2

10

10

10

10

10
_Q>

10

o
\

o
+

I III I I III I

l 0"

-Z. 10

"O

cz

u
^10"4
10"

m
-o

o
\

1
z

10

- 10"'\
o
x>

10"

-3 |

10

<D

___

4.T3

^v.

_K
10

10
-5

10

10

10

10

-6

10

10

10

I , LI,I,

I , I.I.L

40

10

10

'

da/dN (10_6in/cycle)

Life Prediction Ratio Summary


i

0.

40

100

da/dN (10_6in/cycle)

AK (KsiVin)

1.71
2.07
4.35
8.25
15.4
22.2

18.93 (min)
20.
25.
30.
35.
37.87 (max)

RMS %
Error
1.70

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'

i 11in

100

.5 .8

1.25

RMS %
Error

2.
Figure 5.8.3.1.2
5-66

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

INCONEL 625
Condition/Ht: MA
Form: 1 in. Plate
Specimen Type: CT
Orientation:
Stress Ratio: 0.05
Frequency: 10 Hz

Yield Strength: 65.9 ksi


Ult. Strength: 132.9 ksi
Specimen Thk: 0.443 in.
Specimen Width: 2.002 in.
Ref: HD005
(1 of 1)

AK (MPaVin)
4
CT|

10

AK (MPaVin)
4

40
100
i I i I i|i|

I I Mil

Environment: Lab Air; R.T.

10

' I M'l'l

40

100

' I M'l'l

10
10

10

10

10
10

10
2

-Jio~2

-^icf
o

o
\

o 10

o 10

_c

10"3E
T3

10

^|
10 E

_
10

10

-5

^10 >

"O

T3

10

10

10

10
10

10

10

10
10

I I i I ill
40
100

' i i i im

10

10

AK (KsiVin)

da/dN (10'6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary

0.

da/dN (10"6in/cycle)

AK (KsiVin)

3.01
7.20
14.3
25.1
40.8
94.8

20.25 (min)
25.
30.
35.
40.
49.76 (max)

i i i UM
40
100

i i 11in
4
10

AK (KsiVin)

RMS %
Error
3.26

10

.5

.8

1.25

RMS ss
Error

Life Prediction Ratio Summary


i

0.

2.
Figure 5.8.3.1.3
5-67

.5

.8

1.25

INCONEL 718

GO

a
OJQ

o
a

c
o

a >

c
v
S

P*

ft

CO

a >

id

<

H
03

3s
IS
S fa

bo

EU

5-68

INCONEL 718

CO
V

CO

iliiii
OS

IS

PS

5-69

INCONEL 718

CM

AS
::B3:; .N:
:

ivffift-xiaiiil'X

04
05

SI
S3
o
Pi

b.

03

O
b.

b.

t-H

*-4

U
b.

O
E-

a
w
o

U
b.

CO
BS

X
b.

CO
03

b.

b.

1Q

CO

I
5-70

INCONEL 718

tu

o
f :s;S*

CPVi

to

9
3

I
Hi

O
Q

5-71

ESrCONEL 718

'S

II

!:;^;::;

3 I
mm,

SMB

H
0:P3
MHNMMMMMHN

OS
10

3
3

f::::

en
Q

g
CO
OS

fe

5-72

I rNCONEL 718

llilll
05
IO

iH

9
S o
CO H

<1<
.* .
B<
X M SS

-*
882

18

5-73

INCONEL 718

0
i

5-74

INCONEL718

<

1
as

lg

OS
la

['

i
1
I

5
KM

5-75

fa

111

saws

ist;

IB
CO

8* 35

iH

OS

to

a
<

ca

Q
Ed
O
K

IS

I os

<

03
S

1
5-76

CG

S!S*i

11:

ei

MMMMMM*MMMNMMMMMMU*M*tMM

OS

I
1

5-77

INCONEL 718

05
N
CO

S:*Sfc>S

wSf

Alii
PS B3

OS

Q
Ed

CO
BS

EK

5-78

INCONEL 718.

'S

Si

fit

01

***

llilll
OS
10

SI

cq

|l

a
a

I
o

I i

I
5-79

INCONEL 718

tu
O

Al

ilii

iBlll

es

ivfljpS ;
111 - in- - -

--

-----

'-'- ' '' - '''J ''

"-

0)
I

%
CO
a
e>

HUI

CO

CO
OS

as
x

C5

5-80

INCONEL718

<*>

llillll

w
iH

:-:-WH-:-:Kiia-:-:-:

&i

<

5-81

INCONEL 718

CO

00

00

CO

oo

CO
CO

CO

CO

CO

CD

is

00

en

'

oi
to

o
o

CD

CO

gi S

sen

CO

en

en

en

sen

ten

CO

CO

ei
o

10

to

eo
IO

CO

IO

en

s
d

CO

CO

OS

ao

ao

to

10

to

&

IO

OS

en
IO

El

ao

s^"

sN

8
.-

CO

CO

-t

CO

CM

to

CN

CN

CN

CO

^f
c4
t-

CO

i
Ei

J
fi

J
Oil

E^
K

E^

E^

CO

CO

&

CN
CO

s s sr^

t-

E-i

E*

IO
en
0"

en
v

"

ii

eo

s
s

CO

CO

o
o

CO
CN

'

o
o

CO

"

<

**

CN

O
O

g 3 t 2 t S
en

en

BB

eo
to

CO

e-

OS

CN
CO

CO

so s

IN

CO

to

en

to

CO

CO

CO

E"
U

E-<

IO

so

en
to

,-

OS

8
^

**

*-

OS

OS

fN

en

e-

hJ

to
o

to
to

ii

I"

CO

o
o

s
CO

GO

CO

CD

'

04
05
to

2
33

g g g

E-

w
a.

id

s*
s

HH

Si*

Sg
8? 8
8

gas:

BE-

B*
g=
o

CO

c
'Si

&<

g
8

gs

fa
s
CO

Oi

**

*"*

CO

**

CO

CO

r*

""

"

e-

CD

IO

eo

to

CO

eo

<M

IO

IO

o
o

E*

J)

J
E

E*

J
Ei

J)

t"'

fr!

CO

CO

05

CO

CO

eo

CO

CO

CO

"
bo
c

bo

be

be

a
(2

So
-<

I"

3S

ii

as K

to

to
IO

"*

P
&.

So
i B g

CO

J)

01
CO

en

1
3

SB 5?
s*

en
IO

be
c

BS

&

s
S
&
to

<
=t

<
&

ES

fa
CO

5-82

<
B

<:
V:

<
fe

s
fe

e>

en

en
CO

IINCQNEL718

go

rf

rf;

tJS

is
w

^5 .

I*

CO
-4

12
O
U

33

II*
id
1-5*

9||
ug

Q
EU

ill
D O. ?

5-83

INCONEL 718
K

u
b

5>

*a8

3li
'8>
8

Si
ess

OS E

B?

IH

Q
H

5 = "
Bos)

ii*

o
w

0.

CD

9pi
*"
J

a
P

a
a
u

a
a
0.

2
Q

5-84

INCONEL 718
at

2>

is
rf

*&
go

4'3

lij
s 5 <?
|5

00
-t

HI

O
O

3
E8
8

a.
so

i*
9*5
Id B

es eafc
2
a
Q
o

111
5

5-85

MCONEL718.
6S

l
5>

rf

^'4

is

1i

I*'

Be

so
t

55
in
Eh

II'
- "o CO

i*

CO

9??

u OS
- O

&

BS

fi7
s
a
o

5-86

This page intentionally left blank

5-87

\ INCONEL 718
Condition/Ht:
Form:
Specimen Type: CT
Orientation: LT
Frequency: 10 Hz
Environment: LAB AIR; RT

Yield Strength:
Ult. Strength:
Specimen Thk: 0.25 in.
Specimen Width: 2 in.
Ref: NC005
(1 of 1)

AK (MPaVin)
4

10

-I'l

40

I'l'l

AK (MPaVin)
4

100

I I >I'I'l

10

40

-I'l M'l'l

100

' I M'l'l

10
-=

Stress Ratio: 0.1

10

10
10

10

10
O

10'2^
o

frio-4
c
_

10

2 u

io"

o^10~
c
_

10"3E

_i.T3

z. 10

Z. 10
T3

10

- io^\

"a

10

_c I
10
10

10

10

10

10

I , I,I,I,

I , I,I,I,

40

10

10

10
10
4

100

AK (KsiVin)
AK (KsiVin)

da/dN (10"6in/cycle)

Life Prediction Ratio Summary


o
0.

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.0720
0.129
0.498
1.15
2.46
4.86
8.44
13.9
22.3
56.8
145.
374.
612.

9.10 (min)
10.
13.
16.
20.
25.
30.
35.
40.
50.
60.
70.
75.14 (max)

RMS %
Error
17.15

10

AK (KsiVin)

.5 .8

1.25

RMS %
Error

2.

Figure 5.9.3.1.1
5-88

Life Prediction Ratio Summary


-r-

T-

.5

.8

1.25

INCONEL 718
Condition/Ht: 1325F 8HRS
Form: 4 in. Forging
Specimen Type: CT
Orientation: LT
Frequency: 6 Hz
Environment: L.H.A.; RT

FC

Yield Strength: 168 ksi


Ult. Strength: 199 ksi
Specimen Thk: 0.54 - 0.55 in.
Specimen Width: 7.4 in.
Ref: 88579
(1 of 2)

AK (MPaVin)
4

10

40

- i M M'l'i

rI ' I 'I'l'l

10

40

RMS %
Error
7.76

100

40

100

6.54
9.70
19.3
25.6

r-

1.25

da/dN (10"6in/cycle)
1.40
2.17
4.27
7.07
10.9
16.1
34.0
71.4
152.
329.
689.

17.63 (min)
20.
25.
30.
35.
40.
50.
60.
70.
80.
89.46 (max)

1.13
2.38
4.16

.8

' I 'I'l'l

10

AK (KsiVin)

0.393
0.470

.5

100

AK (KsiVin)

Life Prediction Ratio Summary


0.

40

b I ' I 'I'l'l

da/dN (10"6in/cycle)

15.35 (min)
16.
20.
25.
30.
35.
40.
50.
54.42 (max)

10

10

AK (KsiVin)
AK (KsiVin)

(2 of 2)

AK (MPaVin)
1

100

- Stress Ratio: 0.08

TO 1150F

2.

RMS %
Error
11.73

Figure 5.9.3.1.2
5-89

Life Prediction Ratio Summary

0.

.5

.8

1.25

2.

I INCONEL 718 I
Condition/Ht: 1325F 8HRS
Form: 4 in. Forging
Specimen Type: CT
Orientation: TL
Frequency: 6 Hz
Environment: L.H.A.; RT

FC

Yield Strength: 166 ksi


Ult. Strength: 197 ksi
Specimen Thk: 0.51 in.
Specimen Width: 6.01 in.
Ref: 88579
(1 of 1)

AK (MPaVin)
- I

4
10
I >lllll

100
10

10

10
2

io"

o
\

_0J

u
^10"4
-3 |

-3 |

~~
_

10

-5

ho

xi

10

-5

_^"o
10

10

_K I10

10
10

10

10

10

10

40

10

2L 10

~o

10

' I 'I'l'l

10

10

-a

b I

-= 10

ID"3

\
c

AK (MPaVin)
4

40
100
I I llll'l
-I

Stress Ratio: 0.08


10

TO 1150F

- I , U.I,
4

10

10

I , I,LI,

10

40

10

i i

100

da/dN (I0*6in/cycle)

Life Prediction Ratio Summary

0.

da/dN (10"6in/cycle)

AK (KsiVin)

1.65
2.68
5.10
8.98
14.4
30.9
60.4
113.
265.
822.

21.31 (min)
25.
30.
35.
40.
50.
60.
70.
80.
86.24 (max)

RMS %
Error
8.08

i i i nil
40
100

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

LL

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


i

0.

2.

Figure 5.9.3.1.3
5-90

.5

.8

1.25

INCONEL 718
Condition/Ht: 1750F
Form: 0.5 in. Plate
Specimen Type: CT
Orientation:
Stress Ratio: 0.05

1HR

Yield Strength: 147.9 ksi


Ult. Strength: 191.3 ksi
Specimen Thk: 0.298 - 0.49 in.
Specimen Width: 1.153 - 1.998 in
Ref: HD016
(1 of 2)

AK (MPaVin)
1

- I

10

' I M'l'l

EF

AC 1325F

(2 of 2)

AK (MPaVin)
1

40
100
Tl I l I l|>l

= I

10

' I M'l'l

40

100

' I M'l'l

Environment: Lab Air; R.T.;


Frequency: 10. Hz

- Environment: Lab Air; 1200T; -=\ 10


_
Frequency: 0.67 Hz

10

10
10
10

o
o 10

o
\

-3 |

10
10

T3

10

10
10
10
10

10

'

I I HU

10

I I I III

40

100

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)

AK (KsiVin)

Life Prediction Ratio Summary

0.

.5

40

100

.8

1.25

da/dN (10"Mn/cycle)
0.132
0.207
0.633

12.11 (min)
13.
16.
20.
25.
30.
35.
40.
45.38 (max)

22.8
24.7
38.5
48.4
63.3

28.72 (min)
30.
35.
40.
45.46 (max)

RMS %
Error
2.74

10

AK (KsiVin)

RMS %
Error

9.80

Figure 5.9.3.1.4
5-91

1.65
3.69
6.88
11.9
20.0
34.7

Life Prediction Ratio Summary


0.

.5

.8

1.25

\ INCONEL 718 I
Condition/Ht: 1750F 1HR
Form: 0.63 in. Forged Bar
Specimen Type: CT
Orientation: T-L
Stress Ratio: 0.05
Frequency: 0.7 Hz

AC 1325F
Yield Strength: 164.9 ksi
Ult. Strength: 208.1 ksi
Specimen Thk: 0.3 - 0.302 in.
Specimen Width: 1.152 - 1.153 in
Ref: HD016
(1 of 4)

AK (MPaVin)
4

10

- I i I ii'l'l

40

100

1 ' 1 Tl'l

10
10

.22
io"

10

Q)
O

u
o^10-4

o 10
10

Z 10

E
10

_= I"

~<3

XJ

10

10
10

:
10

10

10

- i , I,I,I,
4

10

i , I,I,I,

10

40

10

"

100

37.80 (max)

RMS %
Error
3.21

.5

.8

_L

10
V

2
10~
o
\

10"
^^
z

m^
u
X)

10

'I

jfcl

ff

-rz 10

I , I,I,I,

I , I,I,I,

40

10

100

da/dN (10"6in/cycle)
1.42
2.66
5.67
11.3
19.2
31.7
53.7
61.6

13.42 (min)
16.
20.
25.
30.
35.
40.
41.21 (max)

Life Prediction Ratio Summary


0.

AK (KsiVin)

1.13
2.00
4.34
8.76
16.0
28.9
40.8

13.90 (min)

I ' I Tl'l

AK (KsiVin)

da/dN (10"6in/cycle)

16.
20.
25.
30.
35.

100

JP
M

AK (KsiVin)
AK (KsiVin)

40

Environment: Lab Air; 800F

10

10

10

- I ' I M'l'l

10

Environment: Lab Air; 600T

(2 of 4)

AK (MPaVin)

1.25

RMS %
Error
2.22

Figure 5.9.3.1.5
5-92

Life Prediction Ratio Summary


0.

.5

.8

1.25

2.

INCONEL 718
Condition/Ht: 1750F
1HR
Form: 0.63 in. Forged Bar
Specimen Type: CT
Orientation: T-L
Stress Ratio: 0.05
Frequency: 0.7 Hz

AC 1325F
Yield Strength: 164.9 ksi
Ult. Strength: 208.1 ksi
Specimen Thk: 0.3 - 0.302 in.
Specimen Width: 1.152 - 1.153 in
Ref: HD016

(3 of 4)
AK (MPaVin)
1
4
10
40
100
i i i mil
I- I i I i I i IM
- Environment: Lab Air; 1000T 10

10

40

10

u
u 10
c

10

Z 10
XI

10

10

10
40

M
W

39.66 (max)

RMS %
Error
3.54

.8

m^
u

10

40

-6

100

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)

20.4
34.4
60.1
82.4
91.2

16.46 (min)
20.
25.
30.
31.33 (max)

RMS %
Error

Life Prediction Ratio Summary


I

.5

I , LI,!,

" I , I,I,I,
4

Life Prediction Ratio Summary


0.

x>

-5
10

2.35
2.34
3.56
7.57
12.1
16.5
21.6
30.3

13.
16.
20.
25.
30.
35.

100

da/dN (I0'6in/cycle)

12.74 (min)

rffl

AK (KsiVin)
AK (KsiVin)

<u

2
o
10~
o
\

10"

10

100

_ I I I llllll
I I I llllll
-I
Environment: Lab Air; 1200T 10

10

(4 of 4)

AK (MPaVin)

1.74

1.25

0.

Figure 5.9.3.1.5 (Concluded)


5-93

.5

.8

1.25

2.

^ INCONEL 718 I
Condition/Ht: 1750F 1HR
Form: 0.63 in. Forged Bar
Specimen Type: CT
Orientation: TL
Stress Ratio: 0.05
Frequency: 8.3 10 Hz

C 1325F
Yield Strength: 164.9 ksi
Ult. Strength: 208.1 ksi
Specimen Thk: 0.301 in.
Specimen Width: 1.151 in.
Ref: HD016
(1 of 1]

AK (MPaVin)
4

10

40

AK (MPaVin)
4
10
1 I l MM

100

40

100

' I 'I'll
10

10

Environment: Lab Air; R.T.

10

10

10

10

10

10

-Jio"2

~"

io"

6^10-4

10

10

-3 I

10

10
10

10

D
XI

10

o
o^10-4

D
X

10

10

10

10

10

10

i , i.i.i,

i , i,i,i,
4

10

40

-6

10

10
10

l i l i 11

100

da/dN (10"6in/cycle)

25.
30.
35.
40.
50.
56.03 (max)

Life Prediction Ratio Summary

0.

100

da/dN (10"6in/cycie)

AK (KsiVin)

1.53
3.08
6.32
11.6
21.6
41.8
116.
235.

16.56 (min)
20.

RMS %
Error
2.00

I i I i li

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

.5

.8

1.25

2.

RMS %
Error

Life Prediction Ratio Summary


i

0.

Figure 5.9.3.1.6
5-94

.5

-i

.8

1.25

INCONEL 718
Condition/Ht: 1750F AC
Form: 0.06 in. Sheet
Specimen Type: CCP (max load specified)
Orientation:
Stress Ratio: 0.05
Frequency: 0.7 Hz
(1 of 1)

AK (MPaVin)
' I 'I'l'l

40

AK (MPaVin)
1

100

' I 'I'l'l

Environment: Lab Air; 600T

10

10

10

10
Q)

o
o 10

Z 10
X!

x>
10

10

10

wJF

10

40

100

I III I-

- I

10

I III

Yield Strength: 174 ksi


Ult. Strength: 204.1 ksi
Specimen Thk: 0.061 in.
Specimen Width: 1.995 in.
Ref: HD017

10

__

10

10
jD

o
6-10-4

o
10

-2

io"2

10

E
-5

-ZL 10
X

10

10

xi

10

10

-zz

1 ,1,1,1,

" 1 , 1,1,1,
4

10

40

10

100

, I,I,I,

10

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

1.50
1.90
3.53
5.73
8.69
13.1
29.2
46.5

Life Prediction Ratio Summary

RMS %
Error

Life Prediction Ratio Summary


i

0.

10

AK (KsiVin)

da/dN (10-6in/cyde)

18.40 (min)
20.
25.
30.
35.
40.
50.
57.54 (max)

RMS %
Error
2.11

, I,I,I,

AK (KsiVin)
AK (KsiVin)

_K I
10

.5

.8

1.25

0.

2.

Figure 5.9.3.1.7
5-95

.5

.8

1.25

\ INCONEL 718 I
Condition/Ht: 1750F AC
1325F
Form: 0.06 in. Sheet
Specimen Type: CCP (max load specified)
Orientation:
Stress Ratio: 0.05
Frequency: 0.7 Hz
(1 of 2)

AK (MPaVin)
4

- I

10

' i 'I'l'l

40

10
_o
o
6^10-+

Z. 10

-a

"o _=
10

10

10

io"

, I,I,I,
4

10

, I,I,I,
40

10

10

\
o
"o

-5

^
10

10

10
10

10

10

'

RMS %
Error
2.79

100

0.

i ' i 'ii
40

100

da/dN (10"6in/cycle)

AK (KsiVin)

11.1
12.1
18.2
23.3
29.6
29.7

23.42 (min)
25.
30.
35.
40.
40.06 (max)

Life Prediction Ratio Summary


.8

10

AK (KsiVin)

2.12
2.26
3.92
6.43
9.79
14.3
30.8
53.2

.5

'

i i 111

da/dN (10"6in/cycle)

19.39 (min)
20.
25.
30.
35.
40.
50.
57.84 (max)

_K I
10

AK (KsiVin)
AK (KsiVin)

-3 p
10 E

10

JP

5-10-4

o
-a

10

10
2

100

' I 'I'l'l

10

_*"0
10

J*
JF

40

10

10

10

' I 'I'l'l

Environment: Lab Air; 1000T

10

tz I

_L

' I 'I'l'l

(2 of 2)

AK (MPaVin)

100

Environment: Lab Air; 800T

10

Yield Strength: 174 ksi


Ult. Strength: 204.1 ksi
Specimen Thk: 0.061 in.
Specimen Width: 1.999 - 2 in.
Ref: HD017

1.25

RMS %
Error
2.89

Figure 5.9.3.1.8
5-96

Life Prediction Ratio Summary

0.

.5

.8

1.25

2.

NCONEL 718
Condition/Ht: 1750F AC
1325F
Form: 0.06 in. Sheet
Specimen Type: CCP (max load specified)
Orientation:
Stress Ratio: 0.05
Frequency: 5 Hz
(1 of 1)

AK (MPaVin)
1

- I

10

Yield Strength: 174 ksi


Ult. Strength: 204.1 ksi
Specimen Thk: 0.061 in.
Specimen Width: 1.994 in.
Ref: HD017
AK (MPaVin)
4

40
100
-ii I i I ilil

' I M'l'l

(=T-T>

10

40

MINI
TT

100

' I M'l'l^

10

Environment: Lab Air; R.T.

10

10

10

10

10
10

10
2

10"
o

o
6-10-+
c
_

10

z: 10
xs

10

_c

XI

-a

frio-4

10

"o

.-6

Q)

\
10

-5

10

XI

-
10

10

-5

10

10

10

10

10

10

J_J.

10

10

10

40

da/dN (10-6in/cycle)

100

da/dN (10"6in/cycle)

AK (KsiVin)

3.29
5.26
7.54
10.7
19.8

Life Prediction Ratio Summary


0.

i 11111

40

0.560
1.00
1.95

14.22 (min)
16.
20.
25.
30.
35.
40.
47.95 (max)

RMS %
Error
2.24

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i 111ii

100

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary

0.

2.

Figure 5.9.3.1.9
5-97

.5

.8

1.25

2,

1 INCONEL 718 I
1325F
Condition/Ht: 1750F AC
Form: 0.5 in. Plate
Specimen Type: CT
Orientation:
Frequency: 6.7 Hz
Environment: LAB AIR;1000F
(1 of 2)

AK (MPaVin)
4

10

40

_ I 1 I l{llll
1 1 1
Stress Ratio: 0.33

Yield Strength: 150.5 ksi


Ult. Strength: 191.3 ksi
Specimen Thk: 0.298 - 0.299 in.
Specimen Width: 1.152 in.
Ref: HD015

100

N'i

(2 of 2)

AK (MPaVin)

-L

10

' I M'l'l

40

100

' I M'l'l

Stress Ratio: 0.5

10

10

10

10

10
-3

10

10

_a>
o

-3 |

10

T3

"O

T3

*o

iar\
o
_K
10

10"

_
10

z: 10

~o

6^10-'

b-10-

-5

-u

_fi 10
10

10

10

10

10
1

10

i 1 i 1 ill
4
10

1 , 1,1,1,
40

10

2.31
3.82
8.12

16.
20.

25.
30.

15.1
17.8

31.81 (max)

Life Prediction Ratio Summary


0.

.5

.8

0.641
0.760
1.75
3.36
6.54
10.9
11.7

9.19 (min)
10.
13:
16.
20.
25.
25.68 (max)

1.13

13.

da/dN (10'6in/cycle)

AK (KsiVin)

0.522

10.17 (min)

10

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

i I iI Hi
40
100

i i 11 n

100

AK (KsiVin)

RMS %
Error
3.63

-z.
<
m u

10

'

a>

10" T3

io"

1.25

RMS %
Error
2.27

Figure 5.9.3.1.10
5-98

Life Prediction Ratio Summary


0.

.5

.8

1.25

This page intentionally left blank

5-99

^ INCONEL 718
AC

Condition/Ht: 1750F
Form: 0.5 in. Plate
Specimen Type: CT
Orientation:
Stress Ratio: 0.05
Frequency: 0.7 Hz

1325F
Yield Strength: 150.5 - 156.4 ksi
Ult. Strength: 191.3 - 200.7 ksi
Specimen Thk: 0.299 - 0.497 in.
Specimen Width: 1.152 - 1.999 in
Ref: HD015;HD017
(1 of 4)

AK (MPaVin)
4

10

40
i

(2 of 4)

AK (MPaVin)
4

100

10

-Ml H'l'l

I i I H

40

100

I ' I 'ITI

Environment: Lab Air; 800T

10

10

^10"4

Z. 10
T3
XI

10

10

-7

10
4

10

40

F
s

" I , Ml,I,
4

1.82
16.6
26.5

-r. 10

40

10

-= 10
-

100

1.54
3.24
7.95
15.2
23.7
34.1

46.0

57.1
102.

Life Prediction Ratio Summary


0.

i 1111li

16.56 (min)
20.
25.
30.
35.
40.
44.06 (max)

4.51
9.32

57.98 (max)

RMS 56
Error
24.70

da/dN (10"6in/cycle)

AK (KsiVin)

0.513
0.769

35.
40.
50.

10

AK (KsiVin)

da/dN (I0"6in/cycle)

14.29 (min)
16.
20.
25.
30.

10

AK (KsiVin)
AK (KsiVin)

tr

100

_L

.5

.8

RMS %
Error

6.13

1.25

Figure 5.9.3.1.11
5-100

Life Prediction Ratio Summary


r-

0.

.5

.8

1.25

i
Condition/Ht: 1750F
Form: 0.5 in. Plate
Specimen Type: CT
Orientation:
Stress Ratio: 0.05
Frequency: 0.7 Hz

AC

4
10
I | l|l|!|

(3

of 4)

40
100
I | pH

-L

o 10

_c

10" o
o
10

^E

^io~4
_c

-z.

ZIG"5

4"0

10 \
0

-1

jP

io E^

-z.

Jr

&F

10 >
o
T3

~ 10-

-5

-5

10

10

io"7

10~7

I , LLk

" I , I,I,I,

m"8
1

10

40

-6

-6

10

10

" I , LI,I,

m"8

100

da/dN (10"6in/cycle)

AK (KsiVin)
13.60 (min)
16.
20.
25.
30.
35.
40.
41.58 (max)

RMS %
Error
2.40

16.93 (min)
20.
25.
30.
35.
35.62 (max)

0.

.5

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

1.48
2.30
4.97
11.4
20.9
32.8
47.7
53.2

Life Prediction Ratio Summary


i

I , I,I,I,

10

AK (KsiVin)

AK (KsiVin)

-i

10

<D

\
o

XI

M
LT

-6
10

10-
u

_QJ
O

-L

io"3 *~

-1

10
0)

Q)

100

' I 'I'l'l

io"2

ID"3

40

Environment: Lab Air; 1200T 10

10

-Ml 'I'l'l

10"2

i _

(4 of 4)

AK (MPaVin)

Environment: Lab Air; 1000T 10

/ i 0

Yield Strength: 150.5 - 156.4 ksi


Ult. Strength: 191.3 - 200.7 ksi
Specimen Thk: 0.299 - 0.497 in.
Specimen Width: 1.152 - 1.999 in.
Ref: HD015;HD017

Z10"5

ii\i^wiNr_i_

1325F

AK (MPaVin)
1

IK

.8

1.25

2.

RMS %
Error
4.76

Life Prediction Ratio Summary

0.

Figure 5.9.3.1JLI (Concluded)


5-3 01

10.8
17.8
32.2
53.3
71.5
72.6

.5

.8

1.25

2.

I INCONEL 718 I
EF Condition/Ht: 1750F AC

1325F

Form- 0 5 in. Plate


Specimen Type: CT
Orientation:
Stress Ratio: 0.05

(1 of 2)

AK (MPaVin)
4

10

40

8HRS FC TO 1150F HELD 18HRS AC


Yield Strength: 150.5 - 156.4 ksi
Ult. Strength: 191.3 - 200.7 ksi
Specimen Thk: 0.298 - 0.495 in.
Specimen Width: 1.151 - 1.998 in
Ref: HD017;HD015

100

t= I
-= 10

Environment: Lab Air; R.T.;


_ Frequency: 6.67 Hz

(2 of 2)

AK (MPaVin)
10

40
1

' I M'l'l

100

I M'l'l

- Environment: Lab Air; 1000T ^j 10


_
Frequency: 10. Hz

10

10

10

10

10

10

_0)

io"2
o

^10'4
c

Z 10

-a

10

10

E
T3

10

10
-7

10

10

10

10
10

10

~~

10

O
T3

10

10

I , I .I.I.

~ I , I,!,!,
4

10

40

10
4

100

da/dN (10"6in/cycle)

AK (KsiVin)

1.77
3.63
6.76
11.6

18.2
42.5
96.7

50.
58.21 (max)

RMS %
Error
2.68

Life Prediction Ratio Summary


i

.5

.8

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.658
0.688
1.80
3.16

12.91 (min)
13.
16.
20.
25.
30.
35.
40.
44.45 (max)

0.426
0.764

14.19 (min)
16.
20.
25.
30.
35.
40.

10

AK (KsiVin)

AK (KsiVin)

1.25

RMS %
Error
4.61

Figure 5.9.3.1.12
5-102

5.60
10.7
20.1
31.9
46.0

Life Prediction Ratio Summary


a
.5

.8

1.25

INCONEL 718
Condition/Ht: 1750F AC
1325F
Form: 0.5 in. Plate
Specimen Type: CT
Orientation: L-T
Frequency: 0.7 Hz
Environment: LAB AIR;1200F

10

- i i M'l'i

Yield Strength: 150.5 ksi


Ult. Strength: 191.3 ksi
Specimen Thk: 0.477 in.
Specimen Width: 1.997 in.
Ref: HD015

(1 of 1)

AK (MPaVin)

AK (MPaVin)
4

40
100
Ti I i I i|i|

10

40
100
I I I Mill

I Tl'l

10

10

Stress Ratio: 0.03

10

10

10

10
10

10

_a>
o

.2>
o

6^1 o"

-1010

10

10

E
"o

_x"U

10

o
-a

TD

10

-5

-Jio >
XI

.-

10

10

10

10
10

10

10

10
'

I I I III
4
10

10

10

I I 11 ll

40

'

I i I

100

da/dN (10"6in/cycle)

100

da/dN (10*6in/cycle)

AK (KsiVin)

158.

Life Prediction Ratio Summary

0.

40

9.30
17.7
31.8
47.6
69.7
125.

20.23 (min)
25.
30.
35.
40.
50.
55.76 (max)

RMS %
Error
2.05

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

' I ' in

MI

.5

.8

RMS %
Error

Life Prediction Ratio Summary


i

1.25

.5

2.

Figure 5.9.3.1.13
5-103

.8

1.25

2.

I INCONEL 718 I
1325F

Condition/Ht: 1750F AC
Form: 0.5 in. Plate
Specimen Type: CT
Orientation: LT
Frequency: 6.7 Hz
Environment: LAB AIR;800F

Yield Strength: 150.5 ksi


Ult. Strength: 191.3 ksi
Specimen Thk: 0.477 - 0.478 in.
Specimen Width: 1.996 in.
Ref: HD015
(1 of 2)

AK (MPaVin)
1

- I

10

I I "I'l'l

40

100

10

40

100
i I MM

' I M'l'l

(2 of 2)

AK (MPaVin)

Stress Ratio: 0.33

10

nj

10

10
_a;
o

o 10

~"~

10

_x"
10 a

10

"o

_c
10
10

10

10

10

, 1,1,1,
4

i 1 i 1 ,li

10

40

100

da/dN (10"6in/cycle)

AK (KsiVin)
16.
20.
25.
29.34 (max)

0.

.5

.8

0.147
0.220
0.362
0.548
1.39
2.68

9.
10.
13.
16.
20.
23.56 (max)

100

7.32 (min)
8.

Life Prediction Ratio Summary


i

40

da/dN (I0"6in/cycle)

AK (KsiVin)

0.499
1.00
2.08
4.40
8.86
14.1

10.68 (min)
13.

RMS %
Error
2.61

10

AK (KsiVin)

AK (KsiVin)

1.25

2.

RMS %
Error
4.79

Figure 5.9.3.1.14
5-104

5.14
8.10

Life Prediction Ratio Summary

0.

.5

.8

1.25

2.

Condition/Ht: 1750F AC
1325F
Form: 0.5 in. Plate
Specimen Type: CT
Orientation: L-T
Frequency: 6.7 Hz
Environment: LAB AIR;1000F
(1

AK (MPaVin)
4

1
_

10

40

M|l|

Yield Strength: 150.5 ks i


Ult. Strength: 191.3 ksi
Specimen Thk: 0.479 in
Specimen Width: 1.993 n.
Ref: HD015

of 1)

AK (MPaVin)

-L

10

- Stress Ratio: 0.67


"~~

100

| <|l|l|

vICONEL 71<3J 1' P

IN

= I

10

' I 'ITI

40

100

' I 'ITI

10

10"2

IQ"2

-1

-1

10

10

io-3

io"2

-z.

2 10"5

-3|
10
E
^-^
2

10

10

\
c
^^

10

XI

XI

-6
10

~~-^
XI

X)

" 10~-

-5

10

io-7

-6

-6

10

10

~ 1 , 1,1,1,

m"8
1

I , I , I.!,

10

40

m"8 "

100

I , I,I,I,

! , I,I,I,

40

da/dN (10"6in/cycle)

7.74 (min)
8.
9.
10.
13.
16.
18.84 (max)

RMS %
Error
2.29

0.

100

6
da/dN (10 " in/cycle)

AK (KsiVin)

0.531
0.591
0.848
1.16
2.50
3.95
6.13

Life Prediction Ratio Summary


i

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

>
O

-s
10

io"7

io"2

2 10"5

a;
o
u 10
\
c

0)

\
o
"

io"3

0)

.5

.8

1.25

2.

RMS %
Error

Life Prediction Rati<3 Summary


0.

Figure 5.9.3.1.15
5-105

.5

.8

1.25

2.

^ INCONEL 718 H
1325F

Condition/Ht: 1750F AC
Form: 0.5 in. Plate
Specimen Type: CT
Orientation: LT
Stress Ratio: 0.05
Frequency: 0.7 6.7 Hz

Yield Strength: 150.5 ksi


Ult. Strength: 191.3 ksi
Specimen Thk: 0.476 - 0.478 in.
Specimen Width: 1.996 - 1.998 in
Ref: HD015
(1 of 2)

AK (MPaVin)
4

10

(2 of 2)

AK (MPaVin)
4

40
100
i I i I MM

10

10

40

100

I ' I 'I'l'l
I r 'I'l'l -1
Environment: Lab Air; 1000T

10

10
o

z 10"
2

10~

-I

b^io-4
c

10

10

10

40

i "n

J^

, I, I,I,
4

100

RMS %
Error
17.42

Life Prediction Ratio Summary


o

0.

.5

.8

10

I J,l.
40

100

da/dN (10*6in/cycle)
1.52
1.79
3.62
7.18
12.5
19.9
29.8
59.2
106.
113.

15.20 (min)
16.
20.
25.
30.
35.
40.
50.
60.
61.27 (max)

18.8
30.1
68.5
107.

56.07 (max)

AK (KsiVin)

0.781
0.871
2.34
5.62
10.9

16.
20.
25.
30.
35.
40.
50.

10

AK (KsiVin)

da/dN (I0"6in/cycle)

15.64 (min)

z 10

AK (KsiVin)
AK (KsiVin)

z m '\u

10
10

T7

WL

1.25

RMS %
Error
9.25

Figure 5.9.3.1.16
5-106

Life Prediction Ratio Summary


WBti

0.

.5

.8

1.25

2.

Condition/Ht: 1750F
Form: 0.5 in. Plate
Specimen Type: CT
Orientation: L-T
Stress Ratio: 0.05
Frequency: 0.7 Hz

AC

40

1)

AK (MPaVin)
1

100

' I Tl'l

10
,T|

40
|

100
.

rr|

-L

10

Environment: Lab Air; 1000T 10


10~2

ID"2

-1

-i

10

10

/^^

ID"3

io_2

n/cycl

CD

o
\

j
M

^_s

10

,-v

10~3
2

io"
o
\

cu

u 10
\
c

if

Z10"5

~~

X)

\
O

/
XI

E
6

10

E
"^-^
z:

10

>

*y

tW^

Z10"5
D
"

' r

Yield Strength: 129 ksi


Ult. Strength: 160.1 ksi
Specimen Thk: 0.476 in.
Specimen Width: 1.998 in.
Ref: HD015

10

-Ml 'I'l'l

JCONEL 71?3J

1325F

AK (MPaVin)
1

IN

"

10

XI

-6
10

-5

-5

10

10

10-7

ID"7

-6

-6

10

10

"

HA"8

i ,

, I ,l,l,

10

m"6 "

I.I.I,
40

100

1 , 1,1,1,
4

da/dN (10"*in/cycle)

20.36 (min)
25.
30.
35.
40.
50.
60.
66.35 (max)

RMS %
Error
2.80

0.

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

3.96
8.47
15.9
25.3
37.2
78.2
139.
215.

Life Prediction Ratio Summary


i

, I,I,I,

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

1 i

.5

.8

1.25

RMS %
Error

'

Life Prediction Ratio Summary


0.

2.

Figure 5.9.3.1.17
5-107

.5

.8

1.25

2.

-I INCONEL 718 r~
1325F

Condition/Ht: 1750F AC
Form: 0.5 in. Plate
Specimen Type: CT
Orientation: LT
Stress Ratio: 0.05
Environment: LAB AIR; RT

Yield Strength: 150.5 ksi


Ult. Strength: 191.3 ksi
Specimen Thk: 0.477 in.
Specimen Width: 1.998 in.
Ref: HD015
(1 of 1)

AK (MPaVin)
4

10

i ' i 'i'i'i

40

AK (MPaVin)
1

100

I I HIM

= I

10

' I 'I'I'I

40

100

' I 'I'I'I

10

Frequency: 8.33 Hz

10

10
10

10
u
10" E,

z:

Z 10
10

XI

10
10
10
10

10.-8
4

10

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary

0.

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

1.10
1.28
2.68
5.68
10.3
15.7
30.6
37.9

18.26 (min)
20.
25.
30.
35.
40.
50.
54.46 (max)

RMS %
Error
3.72

10

AK (KsiVin)

AK (KsiVin)

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


0.

2.

Figure 5.9.3.1.18
5-108

.5

.8

1.25

This page intentionally left blank

5-109

1 INCONEL 718 h
Condition/Ht: 1750F
Form: Forging
Specimen Type: CT
Orientation:
Stress Ratio: 0.05
Frequency: 0.7 Hz

1325F

AC

Yield Strength: 168.4 ksi


Ult. Strength: 196.7 ksi
Specimen Thk: 0.402 - 0.403 in.
Specimen Width: 1.996 - 1.998 in
Ref: HD017
(1 of 4)

AK (MPaVin)
4

10

40

(2 of 4)

AK (MPaVin)
4
10
I I MUM

100
MUH

40
100
1i I i I MM

Environment: Lab Air; 800T

10

10

<o

10

2 Tt
O

o
\

10~

'
z

m" ^
u
-a

10

10

10

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

AK (KsiVin)

40

0.849

0.993
2.05
4.40
8.32

16.
20.
25.
30.
35.
40.
50.

14.3
22.7
48.6
54.9

51.90 (max)

RMS %
Error
3.60

Life Prediction Ratio Summary


0.

.5

.8

100

da/dN (10"6in/cycle)

15.22 (min)

0.786
1.44
3.28
6.61
11.5
17.4
19.0

16.43 (min)
20.
25.
30.
35.
40.
41.28 (max)

10

AK (KsiVin)

AK (KsiVin)

1.25

RMS %
Error
4.16

Figure 5.9.3.1.19
5-110

Life Prediction Ratio Summary


0.

.8

1.25

INC0NEL 718
Condition/Ht: 1750F
Form: Forging
Specimen Type: CT
Orientation:
Stress Ratio: 0.05
Frequency: 0.7 Hz

AC

1325F
Yield Strength: 168.4 ksi
Ult. Strength: 196.7 ksi
Specimen Thk: 0.402 - 0.403 in.
Specimen Width: 1.996 - 1.998 in
Ref: HD017
(3 of 4)

AK (MPaVin)

(4 of 4)

AK (MPaVin)
4

4
10
40
100
- I I llilll
1 1 1 llilll
-1
Environment: Lab Air; 1000T

= I

10

' I 'I'll

40

100

' I TIM

-Environment: Lab Air; 1200T ~=\ 10


10

10

10

10

10

10
_a>
o

10" ^
o
\

-5

10

10

_K -

10

-7

io"2

o
o 10

-3 |

10

10
"O

jp

10 \
o
XI

,T3

10

-u

10
10

10

10

10

10

10
10

- i , i,i,i,
4

i , 1,1,1,

10

40

'

10

100

da/dN (10"6in/cycle)

RMS %
Error
2.43

.5

.8

100

3.10
4.69
9.37
17.3
28.2
42.3
50.8

14.06 (min)

16.
20.
25.
30.
35.
38.42 (max)

Life Prediction Ratio Summary


0.

llilll

40

da/dN (10"6in/cycle)

AK (KsiVin)

1.24
1.40
3.02
6.04
10.5
18.2
20.8

12.64 (min)
13.
16.
20.
25.
30.
31.19 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'

llilll

1.25

RMS %
Error
4.00

Life Prediction Ratio Summary


0.

Figure 5.9.3.1.19 (Concluded)


5-111

.5

.8

1.25

1 INCONEL 718 h
Condition/Ht: 1750F
Form: Forging
Specimen Type: CT
Orientation:
Stress Ratio: 0.05
Frequency: 10 Hz

1325F

AC

Yield Strength: 168.4 ksi


Ult. Strength: 195.7 ksi
Specimen Thk: 0.402 in.
Specimen Width: 1.998 in.
Ref: HD017
(1 of 1)

AK (MPaVin)
-

4
10
I | >|>|>|

AK (MPaVin)
4

40
100
' | U'l'l

- I

-L

40

100

' I U'l'l

10

Environment: Lab Air; R.T.

10

10

10

~"

10

10

-3

10

10

0)

6^10-+

tD

10

JE
u

10

' I U'l'l

-3 I

10

2 -rz

o 10

10~ |

/
-2L 10

x>

\
a

XJ

10

m^
u

_
_K i
10

10

x>

XI

_R r10

-5

10

10

-7

10

-6

10

10
10

i I i I ill
4

i , i,i,L

10

40

.-8

10

100

da/dN (10"6in/cycle)

AK (KsiVin)

100

da/dN (10"6in/cycle)

AK (KsiVin)

1.93
3.33

6.33
12.0
20.6
40.7
88.8

Life Prediction Ratio Summary

0.

40

0.238
0.925

13.06 (min)
16.
20.
25.
30.
35.
40.
50.
59.94 (max)

9.56

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


-i

0.

2.

Figure 5.9.3.1.20
5-112

.5

.8

1.25

Condition/Ht: 1750F AC
Form: 2 in. Forged Bar
Specimen Type: CT
Orientation: CR
Stress Ratio: 0.05
Frequency: 10 Hz

4
10
i | 'I'l'l

(1

of

1)

-L
10

= I

io"2

\p
0

>'
Z10"5
XJ

o
6^10"+

X)

10"7

I , l,U.

" 1 , 1,1,1,

1rr

10

40

<o

XI

-6

10"7
-6

10

m"8

RMS %
Error
5.64

,40

10

10

-6

100

da/dN (10 "6in/cycle)

AK (KsiVin)

1.36
2.56
4.99
8.81
14.6
21.8
43.7
114.
121.

10

-5

AK (KsiVin)

Life Prediction Ratio Summary


0.

I , I.I,I,

" I , I,I,I,
1

100

^-'
-z.

10

-5

-alE

io

-4.P
10 >
o

10

da/dN (10"6in/cycle)

16.57 (min)
20.
25.
30.
35.
40.
50.
60.
63.69 (max)

-1

AK (KsiVin)
AK (KsiVin)

_L

10

"-'
z io-5
XI
\
o

CT

' I 'I'l'l

io'2

z
-+"
10 \
o

Jff

10

10

4P
m
iff
JfflT

100

(D

\
-3

xa

' I ' I'l'l

40

_
<D

' r

io"3

io"2
PI

10

10

10

-1

Q)
O

\
o
"

__

10"2

o10~*

R
J

AK (MPaVin)
1

Environment: Lab Air; R.T.

io-3

^CONEL 71

Yield Strength: 152.1 ksi


Ult. Strength: 194.4 ksi
Specimen Thk: 0.304 in
Specimen Width: 1.48 in .
Ref: HD017

40
100
' | 'I'l'l

IK

II

1325F

AK (MPaVin)
1

.5

r "'

.8

1.25

2.

RMS %
Error

Life Prediction Ratio Summary


0.

Figure 5.9.3.1.21
5-113

.5

.8

1.25

2.

I INCONEL 718 h
1325F

Condition/Ht: 1750F AC
Form: 2 in. Forged Bar
Specimen Type: CT
Orientation: CR
Stress Ratio: 0.05
Frequency: 0.7 Hz

Yield Strength: 152.1 ksi


Ult. Strength: 194.4 ksi
Specimen Thk: 0.303 - 0.304 in.
Specimen Width: 1.478 - 1.481 in
Ref: HD017
(1 of 4)

AK (MPaVin)
4

10

-Ml Tl'l

40

100

I ' I 'I'l'l

(2 of 4)

AK (MPaVin)
_

_L

10

| ,.|l|

40
|

100

| i|i|<|

-x

10

Environment: Lab Air; 800T

Environment: Lab Air; 600T


-2

10

10

10

10

10
o

io"
o
\

10

5-10-4
c
Z. 10

o
6-10-4

-3 |

-3 |

10

10

XI

10 M
o

_K
10

XI

/
""""

-r: 10 \
D

10

-= 10

10
10

10

10

10
10

10

_0)

- i , I,I,i,
4

10

, I !. I.
40

10

100

da/dN (10~6in/cycle)

35.
40.
50.
56.32 (max)

RMS %
Error
2.02

.5

.8

100

1.72
2.88
6.91
12.9
21.0
31.2
38.3

17.80 (min)
20.

25.
30.
35.
40.
42.93 (max)

Life Prediction Ratio Summary


0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

1.47
2.26
5.30
10.0
16.0
24.2
49.4
78.5

17.61 (min)
20.
25.
30.

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i, i,i,i,

~ i, i ,1,1,

1.25

RMS %
Error
4.92

Figure 5.9.3.1.22
5-114

Life Prediction Ratio Summary

0.

.5

.8

1.25

INCONEL 718
1325F

Condition/Ht: 1750F AC
Form: 2 in. Forged Bar
Specimen Type: CT
Orientation: CR
Stress Ratio: 0.05
Frequency: 0.7 Hz

Yield Strength: 152.1 ksi


Ult. Strength: 194.4 ksi
Specimen Thk: 0.303 - 0.304 in.
Specimen Width: 1.478 - 1.481 in
Ref: HD017
(3 of 4)

AK (MPaVin)
4

10

40

100

- I

10

i I

jT!

40

100

' 1 M'l'l

10

10

:
10
o
6^10"+

_aj

u
u-10-4

o
\

,-s

10

10"3 E

10

2
io~ "

io"3E

10

_K
10

10

_2
io'
2

10

XI

-o

-= 10

,
10

10

-= 10

10

10

-= 10

10
10

-1

- Environment: Lab Air; 1200T -zz 10

Environment: Lab Air; 1000F 10

(4 of 4)

AK (MPaVin)

~ i , i,i,i,
4

10

,;,i,
40

10

da/dN (10"6in/cycle)

25.
30.
35.
40.
50.
55.00 (max)

RMS %
Error
4.05

16.10 (min)
20.
25.
30.
35.
40.
44.50 (max)

Life Prediction Ratio Summary

0.

.5

.8

40

100

1.25

da/dN (10_6in/cycle)

AK (KsiVin)

3.47
7.35
12.7
19.9
31.5
47.6
97.3
158.

16.17 (min)
20.

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i , i,u,

iii
4

100

2.

RMS %
Error
4.63

Life Prediction Ratio Summary

0.

Figure 5.9.3.1.22 (Concluded)


5-115

12.5
21.0
36.4
55.6
76.1
95.3
110.

.5

.8

1.25

2.

i INCONEL 718 I
Condition/Ht: 1750F 1HR Q
Form: 1.13 - 1.3 in. Disk
Specimen Type: KB Bar
Orientation: C-R
Stress Ratio: -0.33
Frequency: 0.3 Hz

1325F 8HR FC TO 1150F AT 100F/HR HOLD 8HR


Yield Strength: 150 ksi
Ult. Strength:
Specimen Thk: 0.251 - 0.255 in.
Specimen Width: 0.903 - 0.911 in
Ref: GE005
(1 of 5)

AK (MPaVin)
4

10

-Ml 'I'l'l

40

Environment: Lab Air; 300F

10

10

Jf
M
Jm

10

-o
_fi |
10

10

10

- I

, I,I,I,
4

10

, I,I,I,
40

IQ"3

6-10-4
\
~~~
c
_

m" ^
u
X)

10

Z 10

RMS %
Error
29.13

10

10
10

-8

10

- i , i,i,i,
4

100

i , i,i,i,

10

40

100

AK (KsiVin)
1.06
1.19
2.08
4.42
8.75

14.88 (min)
16.
20.
25.
30.
35.
40.
49.95 (max)

9.46

Life Prediction Ratio Summary


1.25

da/dN (10"6in/cycle)

AK (KsiVin)

14.6
22.8

.8

0.428
0.771
2.54
5.46

.5

_, :

"o

io"2^

10

da/dN (10"6in/cycle)

18.27 (min)
20.
25.
30.
35.
40.
46.06 (max)

_L

10

AK (KsiVin)
AK (KsiVin)

100

' I 'I'l'l

10

40

10

10

&s

10

' I 'I'l'l

Environment: Lab Air; 600T

10
-=

L_

-5

_L

2
10"
o
\

10~

o
6^10-
\
C

100

I ' I 'I'l'l

(2 of 5)

AK (MPaVin)

2.

RMS %
Error
50.94

Figure 5.9.3.1.23
5-116

15.6
24.9
47.9

Life Prediction Ratio Summary


-I-

.5

.8

1.25

2.

INCONEL 718
Condition/Ht: 1750F 1HR Q
Form: 1.13 - 1.3 in. Disk
Specimen Type: KB Bar
Orientation: C-R
Stress Ratio: -0.33
Frequency: 0.3 Hz

1325F 8HR FC TO 1150F AT 100F/HR HOLD 8HR


Yield Strength: 150 ksi
Ult. Strength:
Specimen Thk: 0.251 - 0.255 in.
Specimen Width: 0.903 - 0.911 in
Ref: GE005
(3 of 5)

AK (MPaVin)
4

10

40
100
Ii I i I U'l

' I 'I'l'l

Environment: Lab Air; 800F

(4 of 5)

AK (MPaVin)
4

1
=q
10

10

40

' I 'I'l'l

100

' I 'I'l'l

Environment: Lab Air; 1000T 10


10
10
-3

10

u
_
6-10-4

10

1.-1

-s

"O

10
10
10
-7

10

10
i I i I Hi

10
4

10

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

50.
50.02 (max)

.5

.8

100

1.25

da/dN (10"6in/cycle)

AK (KsiVin)

0.986
1.67
3.67
7.83

16.
20.
25.
30.
35.
40.

14.4
24.4
40.0
92.9

48.37 (max)

Life Prediction Ratio Summary


0.

40

13.89 (min)

1.20
1.42
2.42
5.00
9.86
17.9
29.7
64.2
64.3

14.17 (min)
16.
20.
25.
30.
35.
40.

RMS %
Error
19.18

10

AK (KsiVin)

AK (KsiVin)

2.

RMS %
Error
9.74

Life Prediction Ratio Summary


i

0.

Figure 5.9.3.1.23 (Continued)


5-117

.5

.8

1.25

2.

^ INCONEL 718 I

Condition/Ht: 1750F 1HR Q


Form: 1.13 - 1.3 in. Disk
Specimen Type: KB Bar
Orientation: C-R
Stress Ratio: -0.33
Frequency: 0.3 Hz

(5 of 5)

AK (MPaVin)
4

10

rrii | i | i|i

40
-l

1325F 8HR FC TO 1150F AT 100F/HR HOLD 8HR


Yield Strength: 150 ksi
Ult. Strength:
Specimen Thk: 0.251 - 0.255 in.
Specimen Width: 0.903 - 0.911 in
Ref: GE005
AK (MPaVin)
4

100

- I

I I I III!

10

40

' I 'I'l'lI

100

' I 'I'l'l=

Environment: Lab Air; 1200T 10


10

10

10

10
-3

10

10

10~

o
o 10

_2>
o

6^10-

10

io"E
10

o
X)

_c

10

10

10

10
10

10

10

10
i

'

i i 11 ii

10

10

i i 11 ii

40

100

da/dN (10-6 in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary

100

da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error

Life Prediction Ratio Summary


i

0.

40

8.13
9.75
16.8
28.8
45.6
65.4
95.9

17.86 (min)
20.
25.
30.
35.
40.
48.27 (max)

19.95

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error

Z 10

10

10

10

.5

.8

1.25

2.

0.

Figure 5.9.3.1.23 (Concluded)


5-118

.5

.8

1.25

2.

This page intentionally left blank

5-119

^ INCONEL 718 I
Condition/Ht: 1750F 1HR Q
Form: 1.13 in. Disk
Specimen Type: KB Bar
Orientation: C-R
Stress Ratio: 0.
Frequency: 0.3 Hz

1325F 8HR FC TO 1150F AT 100F/HR HOLD 8HR


Yield Strength: 150 ksi
Ult. Strength:
Specimen Thk: 0.25 - 0.252 in.
Specimen Width: 0.9 - 0.906 in.
Ref: GE005
(1 of 3)

AK (MPaVin)
4
10
i I I I UN

40
100
1I I I I MM

- Environment: Lab Air; 300T

(2 of 3)

AK (MPaVin)

10

10

' I 'I'l'l

40
100
r~ 'I'l'l

zz.

10
-3

10
2

io"

_0
O

10

<u

-2 TX
u

10"

-3 I

10

z: 10
"a

10

10

6-10-4

_L

Environment: Lab Air; 600T

10

zz

_^"o
10
o
-5

10

10

10

10

10

10
4

10

40

I , i , l.l,
4

100

da/dN (I0~6in/cycle)

RMS %
Error
16.69

.5

.8

I.I.I.
40

100

da/dN (10'6in/cycle)
0.655
0.682
1.59
3.84
7.72
13.2
20.0
23.6

15.82 (min)
16.
20.
25.
30.
35.
40.
42.52 (max)

Life Prediction Ratio Summary


0.

10

AK (KsiVin)

0.456
0.592
1.46
3.28
6.27
11.1
18.8
28.5

15.09 (min)
16.
20.
25.
30.
35.
40.
44.05 (max)

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

1.25

RMS %
Error
13.10

Figure 5.9.3.1.24
5-120

Life Prediction Ratio Summary


r"

0.

.5

.8

1.25

INCONEL 718
Condition/Ht: 1750F 1HR Q
Form: 1.13 in. Disk
Specimen Type: KB Bar
Orientation: C-R
Stress Ratio: 0.
Frequency: 0.3 Hz

(3 of 3)

AK (MPaVin)
4
10
c=ii I i lilt

1325F 8HR FC TO 1150F AT 100F/HR HOLD 8HR


Yield Strength: 150 ksi
Ult. Strength:
Specimen Thk: 0.25 - 0.252 in.
Specimen Width: 0.9 - 0.906 in.
Ref: GE005
AK (MPaVin)
1

40
100
-1I I 11 INI

4
10
r=i> i i MIII

40
100
I I I I IUI
10

- Environment: Lab Air; 1000T 10

10

10

10

10

10

o
u 10

o
o 10
c

r=M0 '
10

-5

-o

10

"O

10

-=|10

-o
10

10

_K

>
-o

10
10

10

-7

10

10

10

10

40

da/dN (10'6in/cycle)

16.
20.
25.
30.
35.
40.
45.99 (max)

Life Prediction Ratio Summary


0.

da/dN (10"6in/cycle)

AK (KsiVin)

1.17
1.73
3.32
5.86
11.4
18.7
29.4
45.0

14.92 (min)

RMS %
Error
7.64

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I I I I III
40
100

I I II I I

100

.5

.8

1.25

i-'

RMS %
Error

Life Prediction Ratio Summary


i

0.

2.

Figure 5.9.3.1.24 (Concluded)


5-121

.5

.8

1.25

2.

-\ INCONEL 718 I
Condition/Ht: 1750F 1HR Q
Form: 1.13 - 1.3 in. Disk
Specimen Type: KB Bar
Orientation: C-R
Stress Ratio: 0.03
Frequency: 0.3 Hz

1325F 8HR FC TO 1150F AT 100F/HR HOLD 8HR


Yield Strength: 150 ksi
Ult. Strength:
Specimen Thk: 0.25 - 0.254 in.
Specimen Width: 0.9 - 0.91 in.
Ref: GE005
(1 of 4)

AK (MPaVin)
1

- I

10

I I Min

40

100
a

I I 'l'l'l

10

10

10

40
1

100

M'l'l

-1

Environment: Lab Air; 800T

- I

-= 10

Environment: Lab Air; 300"F

(2 of 4)

AK (MPaVin)
' I M'l'l

10

-3

10

o
o 10

io~

10

10

_qj

10

G-10-
c
z. 10
"o

t:

XI

10 \
o

HZ
4

-3 |

10

II I I

RMS %
Error
5.59

rf

10

- I , I,I,I,
4

100

100

1.25

0.111
0.165
0.240
0.332
0.731
1.36
2.72
5.85

7.10 (min)
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
40.11 (max)

I--

.8

1,1,1.
40

da/dN (10"6in/cycle)

AK (KsiVin)

1.82
1.86
3.98
7.94
14.3
23.4
40.8

.5

10

AK (KsiVin)

Life Prediction Ratio Summary


0.

m~ ^
u

10

da/dN (10"6in/cycle)

19.86 (min)
20.
25.
30.
35.
40.
47.23 (max)

^-^

AK (KsiVin)
AK (KsiVin)

'I

10

I , I,I,I,
40

10"

T3

10
10

<D

10"
o
\

10

10

10

10

_oj

2.

RMS %
Error
15.90

Figure 5.9.3.1.25
5-122

12.3
23.9
35.9
36.1

Life Prediction Ratio Summary


i

.5

.8

1.25

INCONEL 718
Condition/Ht: 1750F 1HR Q
Form: 1.13 - 1.3 in. Disk
Specimen Type: KB Bar
Orientation: C-R
Stress Ratio: 0.03
Frequency: 0.3 Hz

1325F 8HR FC TO 1150F AT 100F/HR HOLD 8HR


Yield Strength: 150 ksi
Ult. Strength:
Specimen Thk: 0.25 - 0.254 in.
Specimen Width: 0.9 - 0.91 in.
Ref: GE005
(3 of 4)

AK (MPaVin)
4

- I

10

I I >lllll

40

100

-1

' I 'I'l'l

(4 of 4)

AK (MPaVin)
"1

10

I I I I IM

40
1

100

| i | I |i

Environment: Lab Air; 1000T

10

10

10"2^

10

^10"+

J
M

-Z. 10

XJ

10

10"3E
io \
o

10

10

10
10

" I , MJ,
4

I , l,M.

10

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error
21.06

-1

13.

16.
20.
25.
30.
35.
40.
46.60 (max)

.5 .8

100

2.96
2.97
5.13
10.6
22.9
41.6
64.6
87.8
111.

12.99 (min)

Life Prediction Ratio Summary


0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

1.76
2.00
3.56
7.84
14.4
21.0
28.8
65.7

14.19 (min)
16.
20.
25.
30.
35.
40.
49.01 (max)

10

AK (KsiVin)

AK (KsiVin)

1.25

RMS %
Error
22.70

Life Prediction Ratio Summary

Figure 5.9.3.1.25 (Concluded)


5-123

.5

.8

1.25

I INCONEL 718 I
1325F 8HR FC TO 1150F AT 100F/HR HOLD 8HR
Yield Strength: 150 ksi
Ult. Strength:
Specimen Thk: 0.25 - 0.253 in.
Specimen Width: 0.9 - 0.909 in.
Ref: GE005

Condition/Ht: 1750F 1HR Q


Form: 1.13 - 1.3 in. Disk
Specimen Type: KB Bar
Orientation: CR
Stress Ratio: 0.25
Frequency: 0.3 Hz

(1 of 4)

AK (MPaVin)
4

10

' I M'l'l

40

100

10

40
-ii

I ' I Tl'l

"II I l I MM

Environment: Lab Air; 300T

(2 of 4)

AK (MPaVin)
100

i i

Environment: Lab Air; 600T

10

nj

IIIII

10

10

10
o
6-10-4

10
o
"O

-6

10

10

10
4

10

40

100

da/dN (10-6in/cycle)

AK (KsiVin)

RMS %
Error
23.83

6.03
12.1
13.4

.5

.8

1.25

100

1.36
2.67
6.83
13.8
24.3
32.8

17.33 (min)
20.
25.
30.
35.
38.01 (max)

Life Prediction Ratio Summary


0.

40

da/dN (10~6in/cycle)

AK (KsiVin)

0.373
0.465
0.949
2.53

13.99 (min)
16.
20.
25.
30.
35.
35.84 (max)

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error

16.68

2.

Figure 5.9.3.1.26
5-124

Life Prediction Ratio Summary


0.

.5

.8

1.25

2.

NCONEL 718
Condition/Ht: 1750F 1HR Q
Form: 1.13 - 1.3 in. Disk
Specimen Type: KB Bar
Orientation: C-R
Stress Ratio: 0.25
Frequency: 0.3 Hz

1325F 8HR FC TO 1150F AT 100F/HR HOLD 8HR


Yield Strength: 150 ksi
Ult. Strength:
Specimen Thk: 0.25 - 0.253 in.
Specimen Width: 0.9 - 0.909 in.
Ref: GE005
(3 of 4)

AK (MPaVin)
4

10

40

100

- I I I11' I 'I
I ' I 'I'l'l
Environment: Lab Air; 800F

(4 of 4)

AK (MPaVin)
I

10

10

' I 'I'l'l

40

" '1

100
a

'I'l'l

Environment: Lab Air; 1000T


10

10

~~

10

-3

10

10

10

6-10-*

10

"O

_K

10

z: 10

_K -

-o

10

10

10

10

10

10

Mil,
4

I , I,I,I,

10

40

10

I , UJ,
4

100

da/dN (10"*in/cycle)

16.
20.
25.
30.
35.

Life Prediction Ratio Summary


0.

.5

.8

100

1.63
1.80
2.89
5.80
13.0
25.5
43.8
45.3

12.17 (min)
13.

35.35 (max)

RMS %
Error
15.48

Mil,
40

da/dN (10"6in/cycle)

AK (KsiVin)

1.36
1.41
2.91
6.95
14.4
21.3

15.78 (min)
16.
20.
25.
30.
33.30 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10
-a

" I ,

-3^

10

10

&
o

\
10

-Z. 10

10

1.25

2.

RMS %
Error
22.77

Life Prediction Ratio Summary


i-'

0.

Figure 5.9.3.1.26 (Concluded)


5-125

.5

.8

1.25

2.

\ INCONEL 718 I
Condition/Ht: 1750F 1HR Q
Form: 1.13 - 1.3 in. Disk
Specimen Type: KB Bar
Orientation: C-R
Stress Ratio: 0.54
Frequency: 0.3 Hz

1325F 8HR FC TO 1150F AT 100F/HR HOLD 8HR


Yield Strength: 150 ksi
Ult. Strength:
Specimen Thk: 0.25 - 0.255 in.
Specimen Width: 0.902 - 0.922 in
Ref: GE005
(1 of 5)

AK (MPaVin)
4

- I

10

40

'I M'l'l

ID"3

.22

o 10

Z 10

10

10

' I M'l'l

10

10

"

M
w
m

fi

, I,I,I,
4

I , I,LI,

10

40

100

Environment: Lab Air; 300F

_i

10
_0J

2
10"
-3 I
10 E

10 o

10

10

4
10
er-1i I i !' I > I

23.59 (max)

RMS %
Error
41.56

.5

.8

10

10

.22

u
4

6^10-

10

"o

10

10

"o

o
T7

_-6R -

10

-5

10

10
10
'

10

i i i' ii

100

10

40

i I Hi
100

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)

1.08
1.07
1.97
3.63
9.65

12.93 (min)

13.

16.
20.
23.39 (max)

Life Prediction Ratio Summary


0.

10

0.643
0.555
0.934
3.59
5.83

16.
20.

100

I I I i IM

10

da/dN (10"6in/cycle)

12.37 (min)
13.

40
i

Environment: Lab Air; 600F

AK (KsiVin)
AK (KsiVin)

(2 of 5)

AK (MPaVin)

1.25

RMS %
Error
23.62

Figure 5.9.3.1.27
5-126

Life Prediction Ratio Summary


0.

,
.5

,
.8

,
1.25

Condition/Ht: 1750F 1HR Q


Form: 1.13 - 1.3 in. Disk
Specimen Type: KB Bar
Orientation: C-R
Stress Ratio: 0.54
Frequency: 0.3 Hz

4
_

10

| ljl|l|

(3 of 5)

40
|

- I

10

10

<u
2

io"

10

2 10"5

*~
10 \

"O

\
o
" -6
10

100

' I 'I'l'l

-*

D
T>

10

_
_
<D
W2Z

10 E

^-*

z:
- -*?P
10 >
o

o
6-10-4

o 10
c

' I 'I'l'l

40

<U

^^

10

10
-3

(4 of 5)

io~2
-1

<D

I
J
' r

^JCONEL 71

Environment: Lab Air; 1000T -= 10

10

1
_L

10"2

II

AK (MPaVin)

100

| .,.,.,

-- Environment: Lab Air; 800F

IK

1325F 8HR FC TO 1150F AT 100F/HR HOLD 8HR


Yield Strength: 150 ksi
Ult. Strength:
Specimen Thk: 0.25 - 0.255 in.
Specimen Width: 0.902 - 0.922 in.
Ref: GE005

AK (MPaVin)
1

-'

2 10"5

-a
\
o
" -6

"O

10

io"7

I , I,I,I,

~ I , I , i.h

m"8
1

10

40

-5

\I

10

10"7
-6

10

m"8 ~
1

100

I , I,I,I,

I , l,l,l,

40

da/dN (10"6in/cycle)

11.11 (min)
13.
16.
20.
21.92 (max)

RMS %
Error
35.53

1 t

.5

.8

-6

10

100

1.25

da/dN (10"6in/cycle)

AK (KsiVin)
9.26 (min)
10.
13.
16.
20.
22.64 (max)

0.592
1.14
3.30
5.78
9.00

Life Prediction Ratio Summary


0.

-s
10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

2.

RMS %
Error
19.95

Life Prediction Ratio Summary


0.

Figure 5.9.3.1.27 (Continued)


5-127

0.485
0.820
2.22
3.86
8.98
12.6

.5

.8

1.25

2.

1 INCONEL 718 I
Condition/Ht: 1750F 1HR Q
Form: 1.13 - 1.3 in. Disk
Specimen Type: KB Bar
Orientation: C-R
Stress Ratio: 0.54
Frequency: 0.3 Hz

1325F 8HR FC TO 1150F AT 100F/HR HOLD 8HR


Yield Strength: 150 ksi
Ult. Strength:
Specimen Thk: 0.25 - 0.255 in.
Specimen Width: 0.902 - 0.922 in
Ref: GE005
(5 of 5)

AK (MPaVin)
_

10

-3

4
10
I I >lllll

40
100
I I llllll

AK (MPaVin)
_

-I

10

10
:
10

10

10

^
o

6^10c

Z10"5
"D
t:
10

10

10

10

" 1 , 1,1,1,
4

1 , 1,1,1,

10

40

2
io' ^

10

-3 |
10 E

-3 iz

-J

>

"**"
10

"o

10

X!

^r 10

10

10

10

10

~ I , I,I,I,
4

100

I , I,I,I,

10

40

100

AK (KsiVin)

da/dN (10"*in/cycle)

da/dN (10"6in/cycle)

AK (KsiVin)

0.304
0.424
1.47
6.28

8.80 (min)
9.
10.
13.
16.
20.
22.63 (max)

RMS %
Error
30.20

_K I
10

AK (KsiVin)
AK (KsiVin)

:
-a

10

40
100
i | !>!>!
-i

10

Environment: Lab Air; 1200T

""

10

4
10
i I i|i|i|

8.59
14.4
29.7

Life Prediction Ratio Summary


.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


0.

2.

Figure 5.9.3.1.27 (Concluded)


5-128

.5

.8

1.25

This page intentionally left blank

5-129

EF

INCONEL 718
1325F 8HRS
Condition/Ht: 1760F 1HR WQ
Form: 3.6 in. Disk
Specimen Type: CCP (max stress specified)
Orientation: CR
Stress Ratio: 0.

(1 of 4)

AK (MPaVin)
4

10

40

4
t=1r-rr

10

(2 of 4)

AK (MPaVin)

100

I ' I M'l'l
I r I M'l'l
Environment: Lab Air; R.T.;
Frequency: 0.33 Hz

-2

Yield Strength: 171.6 ksi


Ult. Strength: 201.7 ksi
Specimen Thk: 0.08 in.
Specimen Width: 2 in.
Ref: GE008

10

10
T

40
100
1I MIHU

Environment: Lab Air; 1200T; -=\ 10


Frequency: 0. Hz

10
10

10

10
o

~~
CD

o 10
\
c
-Z. 10

io"2

10

o 10
10

T3

10

10

10

10

10

10
10

10

I I I , I ,!.
10

!,l,l<
40

10

RMS %
Error
38.40

0.

1i

.5

.8

1.25

da/dN (10"6in/cycle)

AK (KsiVin)

0.685
1.21
20.1
80.0
311.
916.
1009.

19.03 (min)
20.
25.
30.
35.
40.
41.00 (max)

0.108
0.116
1.01
3.39
6.49
11.9
41.2
236.

Life Prediction Ratio Summary


i

10

AK (KsiVin)

da/dN (10"6in/cycle)

12.93 (min)
13.
16.
20.
25.
30.
35.
39.18 (max)

i I i 11 li
40
100

i i 1111

100

AK (KsiVin)
AK (KsiVin)

XI

10

z: 10

-Jl0 >

10

10

JI

2.

RMS %
Error
18.18

Figure 5.9.3.1.28
5-130

Life Prediction Ratio Summary


i

0.

.5 .8

1.25

I-'

2.

NCONEL 718
Condition/Ht: 1760F 1HR WQ
1325F 8HRS
Form: 3.6 in. Disk
Specimen Type: CCP (max stress specified)
Orientation: CR
Stress Ratio: 0.

10

40

(=-|i I i 11

Yield Strength: 171.6 ksi


Ult. Strength: 201.7 ksi
Specimen Thk: 0.08 in.
Specimen Width: 2 in.
Ref: GE008

(3 of 4)

AK (MPaVin)
' I 'I'l'l

(4 of 4)

AK (MPaVin)
1

100

EF

10

40

-Ml 'I'l'l

100

I ' I 'I'l'l

-1

Environment: Lab Air; 1200T; 10


_ Frequency: 0.33 Hz

Environment: Lab Air; 1200T; 10


_
Frequency: 0.02 Hz
10

10
IQ"3

5-10-4

10

10

10

10
10

40

"
=

9
if

da/dN (10"6in/cycle)

RMS %
Error
20.58

Life Prediction Ratio Summary


i

0.

.5

.8

I , LLI,

10

40

10

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.148
0.713
3.42
9.41
17.0

13.68 (min)
16.
20.
25.
30.
35.
40.
50.
60.
70.
71.33 (max)

8.25
8.94
25.6
63.0
116.
167.
287.
489.
679.
1132.

19.60 (min)
20.
25.
30.
35.
40.
50.
60.
70.
77.64 (max)

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'

" I , LI,I,

10 E

_^_"D
10 D
~~

100

10

1.25

RMS %
Error
20.50

38.6

65.8
89.3
121.
127.

Life Prediction Ratio Summary

Figure 5.9.3.1.28 (Concluded)


5-131

26.5

i-'

.5

.8

1.25

2.

EF

I INCONEL 718 I
Condition/Ht: 1760F 1HR WQ
1325F 8HRS
Form: 3.6 in. Disk
Specimen Type: CCP (max stress specified)
Orientation: CR
Stress Ratio: 0.

(1 of 1)

AK (MPaVin)
4

10

40

- I ' I 'I'l'l

Yield Strength: 171.6 ksi


Ult. Strength: 201.7 ksi
Specimen Thk: 0.25 in.
Specimen Width: 0.6 in.
Ref: GE008

AK (MPaVin)
4

100
1

I ' I M'l'l

10

- I ' I 'I'l'l

40

100

1 ' I 'I'l'l

Environment: Lab Air; 1200T;


_ Frequency: 0.33 Hz

10

10

10
"""*

10

10
-3

10

10
_a>

^ioc:

.-5

Z 10

io"

10"

o
10
c

-3 |

10

10"

10

"

ior\
10

10

10
10

10

10

10
10

- i , i .i.i.
4

i . i.i.i.

10

40

10

100

da/dN (10'6in/cycie)

Life Prediction Ratio Summary


i

0.

40

100

da/dN (I0"6in/cycle)

AK (KsiVin)

0.223
2.30
12.0
24.7
35.7
50.6
68.7
109.
166.

13.48 (min)
16.
20.
25.
30.
35.
40.
50.
58.25 (max)

RMS %
Error
20.72

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

z
1"
'\
u
o

-a

I
I

10

^s

-5

.5

.8

RMS %
Error

Life Prediction Ratio Summary

1.25

0.

2.

Figure 5.9.3.1.29
5-132

.5

.8

1.25

IMTHMn

"71 Q

Condition/Ht: 1800F 1HR Q 1325F 8HRS FC TO 1150F HOLD 8HRS AC


Yield Strength: 169.2 ksi
Form: 4.67 in. Forging
Ult. Strength:
Specimen Type: KB Bar
Specimen Thk: 0.25 in.
Orientation: CR
Specimen Width: 0.6 in.
Frequency: 0.3 Hz
Ref: GE001
Environment: LAB AIR;1200F

AK (MPaVin)
4

- I

10

40

' I 'I'l'l

of 1)

AK (MPaVin)
1

100

' I M'l'l

Stress Ratio: 0.05


lO"2

-L

4
10
i I i |i|i|

40
100
i | > |i|'|

/^^

6^10*
\
c

cT
oF
Jr

v_^

ZIG"5

-3|
10
E

^-N

55

io'2

o
\

-3l

c
^'

10

-z.

TJ
10

>
XJ

10

\
O
"O

"D

10

-5

-5

10

10"7

""*

-6

-6

10

10

10

40

~ 1 , 1,1,1,

m"8

i ,1,1,1,

"I.I , l,l,

m-8

100

da/dN (10"6in/cycle)

AK (KsiVin)
14.80 (min)
16.
20.
25.
30.
35.
40.
50.
55.00 (max)

40

100

da/dN (10'6in/cycle)

AK (KsiVin)

1.52
2.29
5.69
12.0
23.2
42.9
67.9
104.
117.

Life Prediction Ratio Summary


0.

I , I,I,I,

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
18.29

>

-6

10
lO"7

E
'

Z10"5

-6
10

10'3
a>
o
6"10-+

\
o
"

10

10

lO"3

lO"2

-1

-i
10

10

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary

0.

2.

Figure 5.9.3.1.30
5-133

.5

.8

1.25

2.

I INCONEL 718 h
EF Condition/Ht: 1950F AC

1325F
Yield Strength: 161.1 ksi
Ult. Strength: 198.2 ksi
Specimen Thk: 0.49 - 0.491 in.
Specimen Width: 1.992 - 1.997 in
Ref: HD015

Form: 0.5 in. Plate


Specimen Type: CT
Orientation: LT
Stress Ratio: 0.05

(1 of 2)

AK (MPaVin)
4

10

= I ' I Tl'l
-2

40
100
i i ' HIM

Environment: Lab Air; R.T.;


_
Frequency: 8.33 Hz

- I

.
~q

(2 of 2)

AK (MPaVin)

10

-2

10

40

' I TIM

100

' I 'I'll

=>

Environment: Lab Air; 600T;


Frequency: 0.67 Hz

10

10

10

-1

10

10

10

10

o^10-4

6-10-

-3

10

ZZ

10

-5

10

10
10

10

o
"O

_R ~

10

10

10

10
-7

10

10

10

10
'

10
4

10

10

i i 11 ii

40

100

da/dN (10"6in/cycle)

25.
30.
35.
38.4-0 (max)

RMS %
Error
2.89

0.

.8

1.92
3.93
7.66
13.5
21.1
34.8

20.46 (min)
25.
30.
35.
40.
47.52 (max)

Life Prediction Ratio Summary


.5

da/dN (I0"6in/cycle)

AK (KsiVin)

0.998
1.05
1.93
4.02
7.24
10.8

19.66 (min)
20.

I i 11 li
40
100

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

' i i iHI
4
10

1.25

RMS %
Error
2.68

Figure 5.9.3.1.31
5-134

Life Prediction Ratio Summary

0.

.5

.8

1.25

2.

INCONEL 718
Condition/Ht: 1950F
Form: 0.5 in. Plate
Specimen Type: CT
Orientation: TL
Stress Ratio: 0.05

Yield Strength: 161.1 ksi


Ult. Strength: 198.2 ksi
Specimen Thk: 0.49 in.
Specimen Width: 1.996 - 1.998 in
Ref: HD015
(1 of 1)

AK (MPaVin)
1

10

AK (MPaVin)
1

4
10
40
100
- I I <|i|i|
| ' | 'I'H
-1
Environment: Lab Air; 1000T; 10
_ Frequency: 0.67 Hz
-

b I

10

40

' I TIN

100

' I 'I'H

10

10

10

10
10

10
2

io"

u
:
^10"+

-Jio"2

u
_
u^10-4

o
\

-3 |

-3 |

10

10

10

10

TJ

O
X>

"o

10

10

10

-5

Jio \

_fi 10

10

10

10

10

10
10

EF

1325F

AC

" I , LI,I,
4

I , I,l>h

10

40

10

I , 111,
4

100

da/dN (I0"6in/cycle)

Life Prediction Ratio Summary


o
1

0.

100

da/dN (10"6in/cycle)

AK (KsiVin)

4.72
8.12
15.3
25.8
38.2
47.2

21.00 (min)
25.
30.
35.
40.
43.79 (max)

RMS %
Error
11.81

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

' i i im
10

.5

.8

1.25

RMS %
Error

2.

Figure 5.9.3.1.32
5-135

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

{ INCONEL 718 I
Condition/Ht: ANNEALED 1800F 1 HR, AC, 1325F 8 HR, COOLED AT 100F PER HR
TO 1150F, 1150F 8HR, AC
Form: 0.75 in. Plate
Yield Strength: 180 ksi
Specimen Type: CT
Ult. Strength: 218 ksi
Orientation: L-T
Specimen Thk: 0.187 in.
Frequency: 20 Hz
Specimen Width: 1.5 in.
Environment: LAB AIR; RT
Ref:MA016
(1

AK (MPaVin)
40

10

= I

' I 'I'l'l

1)

AK (MPaVin)
1

100
_L

' I 'I'l'l

= I

10

' I 'I'l'l

40

100

' I TIM

-1

10

- Stress Ratio: 0.02

10

-2

10

10

10

10

10

10
_o
o

frl 0"

io" "

-3 IE

10

Z 10

"O
\
o
"

o
o 10
\
c

o
\
10

10

"O

EZ

10

-6
10

rfiF

_K\

10

10
10

10

10

10
.-8

o
x>

10

10

-ATI

10

T3

" I , U,l,

I , I,I,I,
40

10

10
4

100

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


i

0.

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

2.41
0.989
1.75
3.94
5.10

14.12 (min)
16.
20.
25.
25.60 (max)

RMS %
Error
>100.0

10

AK (KsiVin)

.5

.8

1.25

RMS *
Error

2.

Figure 5.9.3.1.33
5-136

Life Prediction Ratio Summary


;

.5

.8

1.25

i-'

2.

INCONEL 718

Condition/Ht: ANNEALED 1800F 1 HR, AC, 1325F 8 HR, COOLED AT 100F PER HR
TO 1150F, 1150F 8HR, AC
Form: 0.75 in. Plate
Yield Strength: 180 ksi
Specimen Type: CT
Ult. Strength: 218 ksi
Orientation: LT
Specimen Thk: 0.187 in.
Frequency: 10 Hz
Specimen Width: 1.5 in.
Environment: VACUUM; RT
Ref: MA016
(1 of 1)

AK (MPaVin)
4

10

40

i | :Mi

AK (MPaVin)
1

100

i | i|.|i|

Stress Ratio: 0.1

b I

10

' I M'l'l

40

100

' I 'I'l'l
10

10

10

10

10

10

10

10~2 "

6-10-4

^10"+
\
c
_

2 10

10

10

10
10
10

I , 1,1.1,
4

10

40

10

i i 1111

100

da/dN (10"6in/cycle)

100

da/dN (10"6In/cycle)

AK (KsiVin)

3.96
6.73
10.9
25.7
26.2

Life Prediction Ratio Summary

0.

I I llll

40

0.415
0.477
1.02
2.15

15.39 (min)
16.
20.
25.
30.
35.
40.
50.
50.21 (max)

RMS %
Error
45.99

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

o
x>

10

10

10

./o

Ill I

10

10

z: 10
"a

r
f

10

-3 |

10_J E

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary

0.

2.
Figure 5.9.3.1.34
5-137

.5

.8

1.25

2.

\ INCONEL 718 I
Condition/Ht: ANNEALED 180F 1 HR, AC, 1325F 8 HR, COOLED AT 100F PER HR
TO 1150F, 1150F 8HR, AC
Form: 0.75 in. Plate
Yield Strength: 155 ksi
Specimen Type: CCP (max load specified)
Ult. Strength: 178 ksi
Orientation: L-T
Specimen Thk: 0.187 in.
Frequency: 0. Hz
Specimen Width: 3 in.
Environment: LAB AIR; 1200F
Ref:MA016
(1 of 3)

AK (MPaVin)
4

10

- I i I Tl'l

40

10

100

1 ' 1 'I'l'l

Stress Ratio: -0.2

(2 of 3)

AK (MPaVin)

- I

i I >|'l'l

40

100

' I 'I'l'l

Stress Ratio: 0.02

-= 10

-1
10

-2

10

10
-3
-3

10

10"

10
JV

fri o-

\
c

Z 10

,_

10

io

o
o^10"4

\
-3l
E

-3 |

-3

-4.

i<r\
o

10
-5

10

-7

10

10

- 1 , 1,1,1,

10

1 , ill

10

100

10

, I , 11 li
10

da/dN (10"6in/cycle)

AK (KsiVin)

i,i.i.i,
40

60.

Life Prediction Ratio Summary


.5

.8

100

0.0488
0.0822
0.124
0.182

44.06 (min)
50.
65.89 (max)

0.

10

da/dN (10"6in/cycle)

AK (KsiVin)

0.0119
0.0367

43.03 (min)
48.81 (max)

-3

AK (KsiVin)

AK (KsiVin)

RMS %
Error
29.03

10

XI

10

.-8

o
\

10

_c
.-s
10

10

2
io"

r-

x>

10

1.25

RMS %
Error
18.22

Figure 5.9.3.1.35
5-138

Life Prediction Ratio Summary


m
0.

.5

.8

1.25

NCONEL 718

Condition/Ht: ANNEALED 1800F 1 HR, AC, 1325F 8 HR, COOLED AT 100F PER HR
TO 1150F, 1150F 8HR, AC
Form: 0.75 in. Plate
Yield Strength: 155 ksi
Specimen Type: CCP (max load specified)
Ult. Strength: 178 ksi
Specimen Thk: 0.187 in.
Orientation: LT
Specimen Width: 3 in.
Frequency: 0. Hz
Ref: MA016
Environment: LAB AIR;1200F
(3 of 3)

AK (MPaVin)
4

10

40

AK (MPaVin)

100

= I

10

Stress Ratio: 0.5

10

' I 'I'l'l

40

100

' I 'I'l'l

-2

10

10
10

10

10
o

5^10"+
\
c
_

_03

,o-I

-3 |

2 10

o
o 10
10

10

10

J10
>

T3

_c -

10

10

10

10

10

10
10
10

i , i,i,i.

" I , I, I, t,
4

10

10

40

10
4

100

da/dN (10"6in/cycle)

AK (KsiVin)

9.83

Life Prediction Ratio Summary


i

0.

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

15.7
23.8
47.5
111.
222.

26.35 (min)
30.
35.
40.
41.09 (max)

RMS %
Error

10

AK (KsiVin)

AK (KsiVin)

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


i-'

2.

0.

Figure 5.9.3.1.35 (Concluded)


5-139

.5

.8

1.25

2.

\ INCONEL 718 I
Condition/Ht: ANNEALED 1800F 1 HR, AC, 1325F 8 HR, COOLED AT 100F PER HR
TO 1150F, 1150F 8HR, AC
Form: 0.75 in. Plate
Yield Strength: 180 ksi
Specimen Type: CCP (max load specified)
Ult. Strength: 218 ksi
Orientation: L-T
Specimen Thk: 0.187 in.
Frequency: 10 Hz
Specimen Width: 3 in.
Environment: LAB AIR; RT
Ref: MA016
f

AK (MPaVin)
1
U-

4
10
i I ' I i Ml

AK (MPaVin)

1)

40

10

40
100
I'M I'l'l

- I

' I 'I'l'l

100

' I 'I'l'l

10

Stress Ratio: -0.2


-2

10

10

10

-1

10

10
10"3

10"

^io"2
o

o
6^10-+

,o-I

Z. 10

, -o
10

jjj

o
\

o
6-10-4
\
,_
c
_
Z 10

\
O
X)

10"

-3 |

10

io~ \
T3

_fi
10

10

10

10

10

10

10
I

10

10

I I llll

10

40

da/dN (10'6in/cycle)

AK (KsiVin)

0.646

16.93 (min)
20.

1.14
2.48
4.59
7.55

25.
30.
32.35 (max)

Life Prediction Ratio Summary


a
0.

100

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

40

10

100

AK (KsiVin)

RMS %
Error
10.08

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


I

0.

2.

Figure 5.9.3.1.36
5-140

.5

.8

1.25

2.

This page intentionally left blank

5-141

1 INCONEL 718 I
Condition/Ht: ANNEALED 1800F 1 HR, AC, 1325F 8 HR, COOLED AT 100F PER HR
TO 1150F, 1150F 8HR, AC
Form: 0.75 in. Plate
Yield Strength: 155 ksi
Specimen Type: CCP (max load specified)
Ult. Strength: 178 ksi
Orientation: L-T
Specimen Thk: 0.187 in.
Stress Ratio: 0.02
Specimen Width: 3 in.
Environment: LAB AIR;1200F
Ref:MA016
(1 of 3)

AK (MPaVin)
40

10

- I

i I i|i|'|

10

100

' | U'l'l

40

_ I I I llll>l
I
Frequency: 1. Hz

10
~=

Frequency: 0.25 Hz

(2 of 3)

AK (MPaVin)
100

' I I'l'l

-i
10
-=

10

10

10

10

2
io" "

10

10
2

10"

10

-3i

fi

z: 10

o
o 10

z: 10
10 \
X

_
-= io E

o
"

10

-6
10

_*xi
10
o
X

10

10

-7

10

10

10

- i ,

I,I,I,

-= 10

10

i ,i,i,i,
40

10

10

- I , I,I,I,
10

100

da/dN (10"6in/cycle)

RMS %
Error
16.07

.5

.8

5.25
8.09
14.3
21.7
33.3
54.9
140.

17.64 (min)
20.
25.
30.
35.
40.
47.54 (max)

Life Prediction Ratio Summary


0.

100

da/dN (10"6in/cycle)

AK (KsiVin)

3.97
5.88
9.69
17.4
16.6

23.08 (min)
25.
30.
35.
38.50 (max)

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , LI,I,

1.25

RMS %
Error
16.64

Figure 5.9.3.1.37
5-142

Life Prediction Ratio Summary


0.

.5

.8

1.25

NCONEL 718

Condition/Ht: ANNEALED 1800F 1 HR, AC, 1325F 8 HR, COOLED AT 100F PER HR
TO 1150F, 1150F 8HR, AC
Form: 0.75 in. Plate
Yield Strength: 155 ksi
Specimen Type: CCP (max load specified)
Ult. Strength: 178 ksi
Orientation: L-T
Specimen Thk: 0.187 in.
Stress Ratio: 0.02
Specimen Width: 3 in.
Environment: LAB AIR;1200F
Ref:MA016
(3 of 3)

AK (MPaVin)
1

10

AK ' (MPaVin)
40

10

40
100
-ii I i I i|i|

100

= I ' I 'I'l'lI ' I Tl'l

- i ' i M'l'ir

10

Frequency: 2.75 Hz

10

10

10

10
10

10

io"2
5N

j io"

6^10-4

o
_
6^10-4

-3 Jr

10

-3 |

10

z: io

10

_.-o
10
o

X3

-A.-0

10
x>

10

_.

10

10

10

10
10

10

10

10

LU

10

I I I I 111
40
100

10

10

da/dN (10"6in/cycle)

AK (KsiVin)
25.
30.
35.
40.
46.96 (max)

Life Prediction Ratio Summary


a
i

0.

100

da/dN (10"6in/cycle)

AK (KsiVin)

4.80
4.82
6.43
10.1
14.4
20.1
42.0

18.39 (min)
20.

RMS %
Error
7.97

40

10

AK (KsiVin)

AK (KsiVin)

.5

.8

1.25

2.

RMS %
Error

Life Prediction Ratio Summary


i

0.

Figure 5.9.3.1.37 (Concluded)


5-143

.5

.8

1.25

I INCONEL 718 I
EF Condition/Ht: ANNEALED

1800F 1 HR, AC, 1325F 8 HR, COOLED AT 100F PER HR


TO 1150F, 1150F 8HR, AC
Form: 0.75 in. Plate
Yield Strength: 167 - 180 ksi
Specimen Type: CCP (max load specified)
Ult. Strength: 196 - 218 ksi
Orientation: L-T
Specimen Thk: 0.187 in.
Stress Ratio: 0.02
Specimen Width: 3 in.
Ref: MA016
f

AK (MPaVin)
10

' I M'l'l

40

2)

10
f^-Ti I I MM

100

' I M'l'l

Environment: Lab Air; R.T.;


Frequency: 4. Hz

(2 of 2)

AK (MPaVin)

10

40
100
I i I MM

Environment: Lab Air; 700T;


Frequency: 6. Hz

10

10

10

10
-3

10

10

-2>

10"

10"

^io"
c
_

10

10~

~~

10

^-'

m" ^
u

X)

10

10

10

10
-7

10

10

10

10

10

10

:z 10
-a
-o

o
\

o
u 10

QJ

2 u

10

"

I , I,I,I,

I , I,I,I,
40

10

'

10

100

58.86 (max)

RMS %
Error
13.84

0.

.8

3.42
4.99
7.68
10.6
21.1
53.6
71.4

27.11 (min)
30.
35.
40.
50.
60.
62.56 (max)

Life Prediction Ratio Summary


.5

da/dN (10"6in/cycle)

AK (KsiVin)

0.8140.918
2.23
3.85
5.77
8.22
16.4
31.9

25.
30.
35.
40.
50.

100

AK (KsiVin)

da/dN (10"6in/cycle)

19.51 (min)
20.

i i 11 ii

40

10

AK (KsiVin)
AK (KsiVin)

i i 11 n

1.25

RMS %
Error
20.26

Figure 5.9.3.1.38
5-144

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

\ INCONEL 718 I-

EF

Condition/Ht: ANNEALED 1800F 1 HR, AC, 1325F 8 HR, COOLED AT 100F PER HR
TO 1150F, 1150F 8HR, AC
Form: 0.75 in. Plate
Yield Strength: 155 - 180 ksi
Specimen Type: CCP (max load specified)
Ult. Strength: 178 - 218 ksi
Orientation: L-T
Specimen Thk: 0.187 in.
Stress Ratio: 0.5
Specimen Width: 3 in.
Ref: MA016
AK (MPaVin)
10

- I

40

' I M'l'l

_L

-3

o 10
c
10
"O

10

10

10

40
100
I I <l>l<l

10

10

10

10
I I >lllll

-I
Environment: Lab Air; 1200T;
-= 10
_
Frequency: 8. Hz

10

- Environment: Lab Air; R.T.;


_ Frequency: 10. Hz

(2 of 2)

AK (MPaVin)

100

M'l'l

'

of 2)

10

10 &
o
\

-3 |
10
E

JT
_w

_x"a
10

o
-a

10

o
6-10-4

2 10
"O

MB

I , LI,I,

, I'.l.l,

40

10

-=:

10

10
10
10

10

- I , LI,I,

.8

I , 1.1,1,
40

10

100

AK (KsiVin)

1.25

da/dN (10"6in/cycle)

AK (KsiVin)

3.88
3.89
7.67
15.2
30.9
47.9
73.9

15.99 (min)
16.
20.
25.
30.
35.
37.55 (max)

1.60
2.97
5.52
10.3
11.6

da/dN (10'6in/cycle)

.5

10

10

Life Prediction Ratio Summary


0.

X!

/
/

100

16.10 (min)
20.
25.
30.
31.91 (max)

RMS %
Error
15.41

-3

AK (KsiVin)
AK (KsiVin)

io"2

T3

10

"

10

10

2.

RMS %

Error
10.71

Figure 5.9.3.1.39
5-145

Life Prediction Ratio Summary


a
i

0.

.5

.8

1.25

2.

i INCONEL 718 I
Condition/Ht: ST 1850F
Form: 4 in. Forged Bar
Specimen Type: CT
Orientation: L-T
Frequency: 6 Hz
Environment: L.H.A.; RT

1360 F 9HRS F/C 1175F


Yield Strength: 160 ksi
Ult. Strength: 192 ksi
Specimen Thk: 0.5 in.
Specimen Width: 5.9 - 6 in.
Ref: 88579
(1 of 2)

AK (MPaVin)
4

10

- I ' I Tl'l

40

I ' I 'I'l'l

10

10

jv

frl 0"+
\
c
_

10

10

10

p
J

r
m
m
a

10

i 1 i 1111
4

1 , 1,1,1,

10

40

100

Stress Ratio: 0.08

_L

-zz

-zz
-

69.11 (max)

RMS %
Error
7.47

.5

E
a

10

XI

10

10

100

10

40

100

AK (KsiVin)

1.25

da/dN (10"6in/cycle)

AK (KsiVin)

0.570
1.16
3.69
7.85
13.3
19.6
33.4
47.1

17.85 (min)
20.
25.
30.
35.
40.
50.
59.27 (max)

r-

.8

100

I I I MM

-3 |

10

Life Prediction Ratio Summary


0.

o
\

0.362
0.834
2.12
3.71
10.2
21.1
34.3

50.
60.

40
1

10

da/dN (10"6in/cycle)

27.73 (min)
30.
35.
40.

10

| I | l|l|

AK (KsiVin)
AK (KsiVin)

(2 of 2)

AK (MPaVin)

2.

RMS %
Error
33.80

Figure 5.9.3.1.40
5-146

Life Prediction Ratio Summary


0.

.5

.8

1.25

1 INC0NEL

1360 F 9HRS F/C 1175F


Yield Strength: 160 ksi
Ult. Strength: 192 ksi
Specimen Thk: 0.5 in.
Specimen Width: 5.99 - 6 in.
Ref: 88579

Condition/Ht: ST 1850F
Form: 4 in. Forged Bar
Specimen Type: CT
Orientation: LT
Stress Ratio: 0.08

AK (MPaVin
4

1
|
1

10

I
1

(1 of 2)

- Environment: L.H.A.: 400T:


_
Frequency: 6. Hz

10

40

100

' I ' I 'l'l

-1

10

10
10

10

ID"3 _

io"2

2 10"S
XJ

10

-6
10

2M0~5

wJ

^"
10

ITT

-6

10

-6

10

" I , I,I,I,

m"8
1

100

40

da/dN (10"6in/cycle)

CD

0.

.5

.8

40

100

1 .25

da/dN (10"6in/cycle)

26.20 (min)
30.
35.
40.
50.
60.
62.69 (max)

Life Prediction Ratio Summary


i

10

AK (KsiVin)

0.175
0.973
2.49
4.59
13.6
28.7
47.1

25.53 (min)
30.
35.
40.
50.
60.
68.07 (max)

RMS %
Error
5.97

I , LLIi

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

-5

10

10~7

-^ 10

I , I 1,1,

~ 1 , 1,1,1,

E
'*-'
z.
-4-P
10 \
o

/
m

T3

\
10

10

"^

-5
10

io"7

b-io-4

-z.

4~
10 \
o
x>
_

io-2

<u

6^1 o"+
^s

io"3

<u

a>
o

-1

-1

m"8

10

' I ' i I'I

Environment: S.T.W.; R.T.;


_
Frequency: 1. Hz

10""2

\
o
~

-1

I 'l'l

II
1

(2 of 2)

AK (MPaVin)

100

40

! 1 1 MM
1
1 1 1

/I r

2.

RMS %
Error
12.61

Figure 5.9.3.1.41
5-147

0.251
0.985
2.56
4.26
11.9
22.5
27.7

Life Prediction Ratio Summary

0.

.5

.8

1.25

2.

I INCONEL 718 I
EF Condition/Ht: ST 1850F

1360 F 9HRS F/C 1175F


Yield Strength: 160 ksi
Ult. Strength: 192 ksi
Specimen Thk: 0.5 - 0.51 in.
Specimen Width: 7.39 - 7.4 in.
Ref: 88579

Form: 4 in. Forged Bar


Specimen Type: CT
Orientation: T-L
Stress Ratio: 0.08

(1 of 3)

AK (MPaVin)
_

4
i I

10
jijM

40
100
i | ITI

100
_L

I ' I 'ITI

10

10

-1

10

10

10

0)

o
6-10-4

_Q)

io"2^
o
\

10*
"~

10

10

_s r-

E
.-5

10

o
"o

40

Environment: S.C.S.; R.T.;


_ Frequency: 1. Hz

10

10

10

- I ' I 'ITI

-L
-= 10

Environment: L.H.A.; R.T.;


_ Frequency: 6. Hz

(2 of 3)

AK (MPaVin)

-5

~~"

10

10

10

i 1 i 1 111
4

10

10

i , i,i,i,

10

40

10

100

33.5
52.1

.5

.8

1.25

100

1.13
2.21
4.19
10.2
25.5
55.1
84.2
143.
268.

31.51 (min)
35.
40.
50.
60.
70.
80.
90.
95.99 (max)

Life Prediction Ratio Summary


0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.339
1.13
3.15
6.22
16.1

26.21 (min)
30.'
35.
40.
50.
60.
67.39 (max)

10

AK (KsiVin)

da/dN (10"6in/cycie)

AK (KsiVin)

I , I,I,I,

~ I , I,I,I,

AK (KsiVin)

RMS %
Error
13.51

-= 10
10

10

10

10

10

10

2.

RMS %
Error
5.30

Figure 5.9.3.1.42
5-148

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

NCONEL 718
Condition/Ht: ST 1850F
Form: 4 in. Forged Bar
Specimen Type: CT
Orientation: T-L
Stress Ratio: 0.08

(3 of 3)

AK (MPaVin)
4

10

EF

1360 F 9HRS F/C 1175F


Yield Strength: 160 ksi
Ult. Strength: 192 ksi
Specimen Thk: 0.5 - 0.51 in.
Specimen Width: 7.39 - 7.4 in.
Ref: 88579

40

100

= I

AK (MPaVin)
4
10
40 100
' I 'I'l'l
1 ' I M'l'l

10

Environment: S.T.W.; R.T.;


_ Frequency: 1. Hz

10

10

10

10

10

10

10

z 10
\
o
-o

io"

a)

-S?

.-o
10 o

T3

o
6-10-4

10

10

10"

o
\
3

'

-z.

10

m" ^
u

_K I
10

2 TT

"O

10

10

10

10

10

10

i , I,I,I,

- i , i,i,i,
4

10

40

10
4

100

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary

0.

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.457
0.655
1.80
3.01
8.23
27.1
39.8
165.
316.

28.93 (min)
30.
35.
40.
50.
60.
70.
80.
81.34 (max)

RMS %
Error
12.70

10

AK (KsiVin)

.5

.8

1.25

RMS ss
Error

Life Prediction Ratio Summary


i-i

0.

2.

Figure 5.9.3.1.42 (Concluded)


5-149

.5

.8

1.25

EF

I INCONEL 718 I
Condition/Ht: ST 1850F
Form: 4 in. Forged Bar
Specimen Type: CT
Orientation: S-L
Stress Ratio: 0.08

1360 F 9HRS F/C 1T75F


Yield Strength: 160 ksi
Ult. Strength: 192 ksi
Specimen Thk: 1 in.
Specimen Width: 3.77 in.
Ref: 88579
(1 of 3)

AK (MPaVin)
4

10

- I ' I 'I'l'l

40

10

100

I ' I Tl'l

Environment: L.H.A.; R.T.;


_ Frequency: 6. Hz

10

40

100

1i I i 11111

Environment: L.H.A.; 400T;


Frequency: 6. Hz

^j 1

10

10

10

10

QJ

10

<p

10
o

5*1 o"4

o^10-4

10

*"

10

10

10
-o

10

i I i imi

10

(2 of 3)

AK (MPaVin)

x>

-=ho
>

_ -

10

10

-5

-5

10

10
-A

-7

10

10

10

10

10

o
-u

10

- i , i. i,i,
4

i 1 i hi
40
100

10

i i iiHI

10

da/dN (10*6in/cycle)

60.

61.11 (max)

0.

.5

.8

100

2.81
3.58
6.71
11.4
26.9
80.1
273.
565.
550.

28.21 (min)
30.
35.
40.
50.
60.
70.
80.
84.76 (max)

Life Prediction Ratio Summary

i 1111

da/dN (10"6in/cycle)

AK (KsiVin)

0.356
1.18
2.82
5.62
10.1
28.6
74.5
82.7

20.07 (min)
25.
30.
35.
40.
50.

RMS %
Error
12.82

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

1.25

2.

RMS %
Error
7.63

Figure 5.9.3.1.43
5-150

Life Prediction Ratio Summary


a
0.

.5

.8

1.25

2.

1 \\\\-^CONEL

71

^3 11

1360 F 9HRS F/C 1175F


Yield Strength: 160 ksi
Ult. Strength: 192 ksi
Specimen Thk: 1 in.
Specimen Width: 3.77 in .
Ref: 88579

Condition/Ht: ST 1850F
Form: 4 in. Forged Bar
Specimen Type: CT
Orientation: S-L
Stress Ratio: 0.08

(3 of 3)

AK (MPaVin)
4

10

- I ' I 'I'l'l

40

AK (MPaVin)

~ Environment: S.T.W.; R.T.;


_ Frequency: 1. Hz

10
'

40

100

i ' i 'i'i'i

-i

10

-2

-1

-1

10

10

ID"3

io-3

io"2

d>

o
o10"+
\
c
-

10-3p
E
[p

j
10

ID"7

^io"4
c

10

-^

Z10"5

>

\
o
",-6
10

in

0)

10"

-z.
X)

-6
10

,-s

03

o
\

zio"s

-5

-5

I , M.L

~ I , U.l,

^n-B

10

40

10
-

io"7

-6

-6

10

m"8

100

da/dN (I0"6in/cycle)

14.37

0.

40

100

6
da/dN (10 " in/cycle)

AK (KsiVin)

0.176
1.00
2.63
4.01
6.82
13.5

Life Prediction Ratio Summary


i

10

AK (KsiVin)

20.92 (min)
25.
30.
35.
40.
43.46 (max)

RMS %
Error

I , LI,!,

~ I , l,l,I,

AK (KsiVin)
AK (KsiVin)

'
z:
"O

10
-

10-*?

10

10

10

- i ' rn'l

10

o
~

100

I ' I 'l'l'l

Lh

"ii

.5

.8

1.25

2.

RMS %
Error

Life Prediction Ratio Summary


0.

Figure 5.9.3.1.4[3 (Concluded)


5-1 51

.5

.8

1.25

2.

1 INCONEL 718 r~
Condition/Ht: STA
Form: 3 in. Forging
Specimen Type: CT
Orientation: LT
Frequency: 15 - 30 Hz
Environment: LAB AIR; RT

Yield Strength: 161.2 - 177.4 ksi


Ult. Strength:
Specimen Thk: 0.244 - 0.254 in.
Specimen Width: 2.002 - 2.005 in
Ref: DA006;DA007
(1 of 3)

AK (MPaVin)
4

10

40
100
I I 11 im

10

40

4
10
i I i 111' I

40

100

10

40

100

100

AK (KsiVin)

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error
55.89

0.

.8

0.00926
0.0149
0.0318
0.0605

4.45 (min)
5.
6.
7.
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
46.73 (max)

Life Prediction Ratio Summary


+
o
m
.5

da/dN (10"6in/cycle)

AK (KsiVin)

0.00991
0.0218
0.381
1.24
2.42
4.11
7.59
14.2
24.5
56.4
121.
252.
313.

9.50 (min)
10.
13.
16.
20.
25.
30.
35.
40.
50.
60.
70.
73.51 (max)

(2 of 3)

AK (MPaVin)

1.25

RMS %
Error
14.60

Figure 5.9.3.1.44
5-152

0.105

0.171
0.263
0.739
1.60
3.51
7.75
15.7
32.5
71.5
163.

Life Prediction Ratio Summary


on
A
i

0.

.5

.8

1.25

2.

NCONEL 718
Condition/Ht: STA
Form: 3 in. Forging
Specimen Type: CT
Orientation: LT
Frequency: 15 - 30 Hz
Environment: LAB AIR; RT

Yield Strength: 161.2 - 177.4 ksi


Ult. Strength:
Specimen Thk: 0.244 - 0.254 in.
Specimen Width: 2.002 - 2.005 in
Ref: DA006;DA007
(3 of 3)

AK (MPaVin)
1

10

40

- I I Tlll
1
Stress Ratio: 0.8

AK (MPaVin)
1

100

1 1 llilll

-1
10

i- I

10

40

' I M'l'l

100

' I Tl'l

10

-2

10

10
"""*
10

10

10
10

o^10c
_

10

b-io-4

-3 |

10

ho

10

_x"D

T3

10

10
~~

10

10

10

10

10

1 I 1 1 1I

10

10

1 , 1.1,1,

10

40

10

100

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)
6.
7.
8.

9.
10.
13.
16.
19.57 (max)

Life Prediction Ratio Summary


IS

RMS %
Error

Life Prediction Ratio Summary


i

0.

da/dN (10"6in/cycle)

AK (KsiVin)

0.0294
0.0410
0.0755
0.122
0.189
0.290
0.449
1.67
7.56
58.6

4.59 (min)
5.

RMS %
Error

I llilll
40
100

I I I I III
4
10

AK (KsiVin)

9.02

_.T3

10

10

.5

.8

0.

1.25

Figure 5.9.3.1.44 (Concluded)


5-153

.5

.8

1.25

2.

1 INCONEL 718 I
Condition/Ht: STA
Form: 3 in. Forging
Specimen Type: CT
Orientation: LT
Frequency: 1 Hz
Environment: DIST WATER; RT
(1 of 2)

AK (MPcVin)
4

10

Yield Strength: 161.2 ksi


Ult. Strength:
Specimen Thk: 0.249 - 0.25 in.
Specimen Width: 2.002 - 2.005 in
Ref: DA007

40

(2 of 2)

AK (MPaVin)
4

100

i l i I MM

10

40
1

' I 'I'l'l

100

1 I I Mill

10

Stress Ratio: 0.8


10

10
10
o

o
10
~a

10

10

O
o

10
-5

10
10
10
'

10
4

10

40

100

da/dN (10-6in/cycle)

RMS %
Error
1.83

0.

.5

.8

100

0.820
2.28
8.42
61.0

10.73 (min)
13.
16.
18.89 (max)

Life Prediction Ratio Summary


i

40

da/dN (10-6in/cycle)

AK (KsiVin)

0.964
2.00
5.62
11.5
20.0
31.8
73.6
183.
267.

17.55 (min)
20.
25.
30.
35.
40.
50.
60.
64.41 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

' i ' i' n

' ' 11 ii

1.25

2.

RMS %
Error
6.15

Figure 5.9.3.1.45
5-154

Life Prediction Ratio Summary

0.

.5

.8

1.25

2.

This page intentionally left blank

5-155

1 INCONEL 718 \Condition/Ht: STA


Form: 3 in. Forging
Specimen Type: CT
Orientation: T-L
Frequency: 5 - 30 Hz
Environment: LAB AIR; RT

Yield Strength: 155.4 - 169, ksi


Ult. Strength:
Specimen Thk: 0.25 - 0.254 in.
Specimen Width: 2.001 - 2.007 in
Ref: DA006;DA007
(1 of 4)

AK (MPaVin)
4

-IM

10

'i'i'i

40

100

-il I l Hill

- I

10

Stress Ratio: -1.

10

10

10

io"2"

10 ^E
-z.

_a;
u
o 10
c
XI

-zz

ff
mff
n
4r

"

I , I , l,l,
4

100

da/dN (10'6in/cycle)

10
=

10

10

.5

.8

100

0.0823
0.304
0.919
1.94

16.
20.
25.
30.
35.
40.
50.
60.

Life Prediction Ratio Summary


a
0.

da/dN (10"6in/cycle)

AK (KsiVin)

3.94
8.68

18.2
32.9
82.1
241.
613.

67.33 (max)

RMS %
Error
7.49

, LI,I,
40

11.12 (min)
13.

0.360
0.686
1.54
2.64
3.87
6.47
29.8
86.9
165.

66.61 (max)

D
X

AK (KsiVin)

AK (KsiVin)

25.
30.
35.
40.
50.
60.

.^-o
10

/A
A
A

__

A
10

-3 |

zz 10

7A
-7

io"2
o

10

16.01 (min)
20.

CDS

10

AK (KsiVin)

_i

10

-n 10

10

40

100

I 'I'i'i

?Jr

10

10

10

XI

40

' I 'I'I'I

Stress Ratio: 0.1

10

10

(2 of 4)

AK (MPaVin)

1.25

2.

RMS %
Error
81.12

Figure 5.9.3.1.46
5-156

Life Prediction Ratio Summary

.5

.8

1.25

NCONEL 718
Condition/Ht: STA
Form: 3 in. Forging
Specimen Type: CT
Orientation: TL
Frequency: 5 30 Hz
Environment: LAB AIR; RT

Yield Strength: 155.4 - 169. ksi


Ult. Strength:
Specimen Thk: 0.25 - 0.254 in.
Specimen Width: 2.001 - 2.007 in
Ref: DA006;DA007
(3 of 4)

AK (MPaVin)
4

- I

10

' I M'l'l

4
10
i I I IHM

40

RMS %
Error
9.55

100

da/dN (10"6in/cycle)

.8

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.0201
0.0293
0.0560
0.0930
0.146
0.224
0.340
0.518
1.87
7.01
17.3

3.56 (min)
4.
5.
6.
7.
8.
9.
10.
13.
16.
18.01 (max)

0.0105
0.0211
0.0441
0.0839
0.148
0.553
1.37
3.13
7.28
16.8
40.9
99.9
183.

.5

10

AK (KsiVin)

Life Prediction Ratio Summary


o

0.

40
100
1I I i I i IM

10

AK (KsiVin)
6.15 (min)
7.
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
4-4.22 (max)

(4 Of 4)

AK (MPaVin)

40
100
-ii i i i nil

Stress Ratio: 0.4

AK (KsiVin)

1.25

RMS %
Error
27.65

Life Prediction Ratio Summary


A

0.

Figure 5.9.3.1.46 (Concluded)


5-157

CD

r-

-i

.5

.8

1.25

1 INCONEL 718 I
Condition/Ht: STA
Form: 3 in. Forging
Specimen Type: CT
Orientation: T-L
Frequency: 1 Hz
Environment: DIST WATER; RT

Yield Strength: 155.4 - 169. ksi


Ult. Strength:
Specimen Thk: 0.25 - 0.252 in.
Specimen Width: 2.003 - 2.005 in
Ref: DA006;DA007
[1 of 2)

AK (MPaVin)
1

- I

10

40

i I 'I'l'l

100

' I 'I'l'l

Stress Ratio: 0.1

(2 of 2)

AK (MPaVin)
10

- I I 'I'l'l

10

40

100

' I 'I'l'l

10

Stress Ratio: 0.8

-2

10

10

-i

~~

10

10

10

_Q3

~~

J
I
i

o
o 10
c

10

10

T3

10

io'

_qj

-n 10"

6^10 10

"**

-= 10"

XI

u
\

1
-z.

-ZL 10
10

i"
'\
u
x>

10

10

10

10

10

10

10

- I , LI,I,

10
1

I ,l,lil,

10

40

10

100

I , I,I,I,

I , I , I,!.

40

da/dN (10"6in/cycle)

RMS %
Error
14.98

0.

.5

.8

1.25

0.403
0.555
0.826
5.08
28.5

8.25 (min)
9.
10.
13.
14.97 (max)

Life Prediction Ratio Summary


ii

da/dN (10"6in/cycle)

AK (KsiVin)

0.951
1.09
2.30
6.21
14.8
29.7
50.4
127.
449.
510.

15.08 (min)
16.
20.
25.
30.
35.
40.
50.
60.
60.84 (max)

100

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

2.

RMS %
Error
12.36

Figure 5.9.3.1.47
5-158

Life Prediction Ratio Summary


o
0.

r-

-I-

.5

.8

1.25

INCONEL 718
Condition/Ht: STA
Form: 3 in. Forging
Specimen Type: CCP (max load specified)
Orientation: L-T
Frequency: 5 Hz
Environment: LAB AIR; RT

10

40
1I

I- I ' I Tl'l

Yield Strength: 177.2 ksi


Ult. Strength:
Specimen Thk: 0.204 in.
Specimen Width: 4.008 in.
Ref: DA006

(1 of 1)

AK (MPaVin)

AK (MPaVin)
4

100

10

40
100
~ii i i I'mm

FT

C=TI

I l I MM

I I Mil

10

10

Stress Ratio: -1

-2

10

10

10

10
10

10
-2

_05
O

o 10

io

10

u
^10-

-3 |

ffil

10

Z. 10

x>

10

-=M >

XI

T3

10

10

10

10
10

10

10

10

10

'

I I I III

10

10

I I I III

40

'

RMS %
Error

da/dN (10~6in/cycle)

Life Prediction Ratio Summary


i

.5

.8

10

40

100

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i i i in

i ' 11H

100

1.25

)-
2.

RMS %
Error

Life Prediction Ratio Summary


i

0.

Figure 5.9.3.1.48
5-159

da/dN (10"6in/cycle)

AK (KsiVin)

.5

.8

1.25

2.

INCONEL 718
.:,;,|.:.:.:.;,:

I.:.-.|,:,;,:.|.: l*I.l*w.|

;,|,;.;.|.:.|.:

llll

'S

<D

to

<>

if? if

is

* 9

Hfl

to

<

i-(

Test
Time
(min)

S 111

to

X SS**?
SSCK

to

8**1*

*>W:*W

M
3

to

to

to

to

05
rH

09

T-l

ill OS
$p
sm

18*
O

00

:*:**:

>::*'$::

00
A

to

o>
1-1

.to

:1I8

r*

*t"'

1-H

CO

to

to

to

O
00

00

00

SSM

03

t-

to

WM

05

m
i$
!-<

00 -ti

mm

to

,00:

")

OS
OS
A

^
IS

111

HA

>-*

8
M

CO

1-H

m 111

iil isifi

00

iH

<*

t-l

I-

Si*:*

Sa

l-H

fH

CJ

CN

m
u

m
u

"Sao

2 2.S

::?*;:

M
9 O
"2 B

OT
05

JS

s 2.S
9

0.
0Q

&

06

.-*.

"*

<

y'*-:

1-1

<

w&

03

evi

Vi&

ViS
(Q

:<<::<<<:

prt

>

::::-::::

<?C3$;

E-

:*K

CO

to

to

iH

1-H

09

&(,

:-<N:

H
in
in I1

S fa "S

a
o

PQ
O

'

".''

llll
:#:::::

mm o

fa

1
w

:ft::

a 1 wm
9

<*

c3

EH

Si!
j35g

t 3
rH

9 .
9 fa

EH

>J

E^

CQ

an

CO

E-i

tJ g

o C
>
o
ftife

&

a?o -o
"50 9
Cond
Heat

O fa Gf&<
TJ

c; (i, p;
SffilOffiH
,_; OS ^ OS

fafe - fe 2

5-160

INCONEL718
t!jmM-Mm>W:-l-!-x-S-i*M

...I,,I..,...,...

's

5S-OS

.0
<w

(M

5>

(3
w

HQ

fe
; *"*

Test
Time
(min)

DO +

:-:-:-x*:

o
o
t00
00
rj<

tt-t

*
s
S

22 c

*go
e

,C
* C

C
TH

V; ;.;",.;;:;. fT* '*''.*:,,

1
1

"""
iSSiSSiSSSSSH:
SiSsiSiffliKssw
S:SSfeg:SSSS
00

sl9S;iiiS

2!
>>
i;S?siSsl
::'SS.'f.- .

:>::>:*::*>:::::*:-:
::;:::;::
::::::::

: : : : : : : : :S:: : : : : : : :

iS|:S:S:S*S:S;5sSsSsS:SsSS:
+
OS

00

mmsmm

*lsi:5lsl;&

llll

i
i

<<>

'

;:::::J'.s:.;..- ::J-

CO

?*

:":-:: ":<=>

. :/: :>-5

1-1

L*~

//

CO

eo

eo
<
o

I-H

::>i :>.': >:i-<

; : : : : : : : : ::::| : : : : : :;: :
::::::;;::-::::::::::::::: : .:.:: :::::;::::;: :::

CM
r-1

I-J

::::-:-:>::

3 = Ho

_,

^'''':<i^:,-W'-:''

!:M:!:|:}:|v}:

'S * -=

00
00

es

mmmmmmm

::;:::::::::::::::*:v**t:*:**rc

^v

rt

o
o
t-

::::::::::::::::::::::-::::::::-:

iviv'v:

tu

o
<&
:...<'"*

gj
<rt

CO

rt
M

i*:*:*:*

CO

Jfc

"
^

Si;*:
P*

::-:++*+:-:

"s3 mmmm%m

lj

.
IN

e -2 2
B b'g

S c S S
ig oo-fi

1st
1

:-:-**-*-KV-S:V

IS

ta
S

e
S

Test
Temp
(F)
o
J*
fc

ei

g
g

OS

IO

SS

iiiii
sli^
J*

6-5

OS

a
a
o

o
fr*

t
00
HO

o (5 o. * S)
ososgosS
f*n ^^ ^^ ""r^ M

'S
o

S
8 *,
S0

OB

hM M^ cn hH 3

rH 00 JS 00 S1

O O O c
00 (N <N c>

g
o

09

5-161

-I NASA IIB-7 P/M I


Condition/Ht: 1650F 16HRS TO
Form: 1.75 in. Disk
Specimen Type: WOL
Orientation: C-R
Stress Ratio: 0.05
Environment: LAB AIR;1200F

10

40

Yield Strength: 208.6 ksi


Ult. Strength: 257.1 ksi
Specimen Thk: 0.5 in.
Specimen Width: 2.5 in.
Ref: PW004
(1 of 2)

AK (MPaVin)
1

2000F 1HR OQ

100

i I ! I MM

|i i i I m

10

Frequency: 0. Hz

(2 of 2)

AK (MPaVin)
10

40
-I

' I 'I'l'l

100

1 I I I Mil

10

Frequency: 0.33 Hz

-2

10

10
10

io~2
o

6^10-

-3 EI

10
o

10

.T)

10

O
XI

10
10
10
10
i i 11 n

i i i i HI

10

10

40

100

da/dN (10-6in/cycle)

AK (KsiVin)

RMS %
Error
73.31

4.74
6.09
15.4
36.7
59.0
91.8
141.
338.
432.

51.24 (max)

T"

.8

100

da/dN (lO^in/cycie)

16.
20.
25.
30.
35.
40.
50.

1303.
3593.
6526.
10084.
16495.
30610.
74742.

.5

40

14.67 (min)

Life Prediction Ratio Summary


0.

AK (KsiVin)

315.

13.30 (min)
16.
20.
25.
30.
35.
40.
45.79 (max)

10

AK (KsiVin)

AK (KsiVin)

1.25

RMS %
Error
16.78

Figure 5.10.3.1
5-162

Life Prediction Ratio Summary


,

0.

.5

.8

1.25

i-'

2.

P/M RENE: 95

u
.a
es

IS

|g?

Bill

O
HM

1
5-163

P/M RENE 95
Condition/Ht: 2080F 1 HR AC
1 600F 1HR AC
Form: 2.5 in. Disk
Yield Strength: 165.7 ksi
Specimen Type: CCP (max load specified)
Ult. Strength: 228.6 ksi
Orientation: C-R
Specimen Thk: 0.08 in.
Stress Ratio: 0.
Specimen Width: 2 in.
Frequency: 0.3 Hz
Ref: GE004
(1 of 1)

AK (MPaVin)
4

10

-Ml M'l'l

40

AK (MPaVin)
4

100

I ' I Tl'l

- I

10

I M'l'l

40

100

' I M'l'l

-2

=
10

10

Environment: Argon; 1200T

10

10

-3

10

_a>

io"2"

_OJ

6^10-4

o 10
10
Z 10

E
Z 10

x
10

"O

10

10
10

10

10

! , I,I,I,

10

10

-=
4

40

10
4

100

da/dN (10"6in/cycle)

35.
4-0.
50.
51.58 (max)

Life Prediction Ratio Summary


-i

24.97

0.

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

1.29
1.94
3.71
5.95
9.11
14.0
35.3
41.3

17.82 (min)
20.
25.
30.

RMS %
Error

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

x>
o

10

XI

10

- i ,i,i,i,

tz

10

10

_03

.5

.8

RMS %
Error

Life Prediction Ratio Summary

0.

1.25

Figure 5.11.3.1.1
5-164

.5

.8

1.25

2.

This page intentionally left blank

5-165

EF

P/M RENE 95
Condition/Ht: 2080F 1HR AC
1600F 1HR AC
Yield Strength: 165.7 ksi
Form: 2.5 in. Disk
Ult. Strength: 228.6 ksi
Specimen Type: CCP (max stress specified)
Specimen Thk: 0.08 in.
Orientation: CR
Specimen Width: 2 in.
Stress Ratio: 0.
Ref: GE008
(1 of 3)

AK (MPaVin)
1

4
10
f=1i I M MM

40
100
i I i I MM

Environment: Lab Air; R.T.;


_
Frequency: 0.33 Hz

(2 of 3)

AK (MPaVin)
4

I
-=) 10

10

10

40

' I M'l'l

100

Tl'l

Environment: Lab Air; 1200T;


Frequency: 0.33 Hz

10

10

o 10

Z. 10

nz

&

10

~
A
A

10

u
\

10

10

10

10

10
4

10

40

I , I, I,I,
4

100

da/dN (10~6in/cycle)

RMS %
Error
24.27

.8

40

100

1.25

da/dN (10"6in/cycle)
0.577
2.67
12.0
25.7
42.0
63.7
159.
517.
2253.
12711.
13214.

17.22 (min)
20.
25.
30.
35.
40.
50.
60.
70.
80.
80.21 (max)

Life Prediction Ratio Summary


.5

,l.l,

10

AK (KsiVin)

0.220
0.400
1.56
5.41
12.2
16.5
31.0
55.2

16.68 (min)
20.
25.
30.
35.
40.
50.
56.41 (max)

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

2.

RMS 55
Error
>100.0

Figure 5.11.3.1.2
5-166

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

P/M RENE 95

EF

Condition/Ht: 2080F 1 HR AC
1600F 1HR AC
Yield Strength: 165.7 ksi
Form: 2.5 in. Disk
Ult. Strength: 228.6 ksi
Specimen Type: CCP (max stress specified)
Specimen
Thk: 0.08 in.
Orientation: CR
Specimen
Width: 2 in.
Stress Ratio: 0.
Ref: GE008
(3 of 3)

AK (MPaVin)
4
10
I I I i mi

40
1

AK (MPaVin)
1

100

10

i- I ' I Tl'l

I I I MU

40

100

1 ' I 'I'l'l

Environment: Lab Air; 1200T; 1


Frequency: 0.02 Hz

10

10

10

10
10

10

-Jio"2
o

6-10-4

6^1 o"+

10 ^E
o

10

T3

-z.

10
10

10

10

10

10

10

10
.-8

10

10

10

40

i i. i
4

100

da/dN (1CT6in/cycle)

948.

76.15 (max)

Life Prediction Ratio Summary


i

0.

da/dN (10"6in/cycle)

AK (KsiVin)

369.
662.

60.
70.

11.29

100

3.45
4.03
14.8
33.9
61.3
97.0
200.

19.55 (min)
20.
25.
30.
35.
40.
50.

RMS %
Error

I I 11II

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'

10

.5 .8

RMS %
Error

Life Prediction Ratio Summary


i

0.

1.25

Figure 5.11.3.1.2 (Concluded)


5-167

.5

.8

1.25

^ P/M RENE 95 I
1600F 1HR AC

Condition/Ht: 2080F 1HR AC


Form: 2.5 in. Disk
Specimen Type: KB Bar
Orientation: CR
Stress Ratio: 0.
Frequency: 0.3 Hz

Yield Strength: 165.7 ksi


Ult. Strength: 228.6 ksi
Specimen Thk: 0.25 in.
Specimen Width: 0.6 in.
Ref: GE008
(1 of 1)

AK (MPaVin)
4

10

10

40

' I M'l'l

100

10

-= 10

Jio
-=

-Z. 10
T3

_e l

_03
o
6^10-4
10

E
Z 10

>

10

-5

10

10

10

10

10

I , I,I,I,
4

10

, I, I,I,
40

10

'

I I I III
40
100

da/dN (10"6in/cycle)

AK (KsiVin)

0.413
0.553
4.05
53.0
301.
615.
630.

Life Prediction Ratio Summary


0.

10

AK (KsiVin)

da/dN (10"6in/cycle)

15.06 (min)
16.
20.
25.
30.
35.
36.31 (max)

RMS %
Error
>100.0

I I 11II

100

AK (KsiVin)
AK (KsiVin)

10
10

CD

T3

10

TO O

10

10

. 10"

10

40
100
I I I I 'HI

10

o 10

-o

10

10

E
c

t I ' I 'I'l'l

Environment: Lab Air; 1200T


~~

10

AK (MPaVin)
1

.5

.8

RMS %
Error

Life Prediction Ratio Summary


0.

1.25

Figure 5.11.3.1.3
5-168

.5

.8

1.25

P/M RENE 95
Condition/Ht: 2100F 1HR
Form: 1 in. Disk
Specimen Type: KB Bar
Orientation: CR
Stress Ratio: 0.05
Frequency: 0.3 Hz

SQ

AT 1000F
Yield Strength: 176.1 ksi
Ult. Strength:
Specimen Thk: 0.25 in.
Specimen Width: 0.6 in.
Ref: GE001
(1 of 1)

AK (MPaVin)
4

- I

10

40

' I M'l'l

AK (MPaVin)
4

100

' I 'I'l'l

10

FT

t=r-1[

I i |i|i

40
100
"1i I i MM
10

Environment: Lab Air; 1200F

10

10

o 10
c
2L 10
o
"O

_fi

10

-7

10

10

"*"

-=

-=

=.
-

"

E
m

XC]
nWB

, I,I,I,
4

10

, I , I.I,
40

10
10

10
-3

10
2

10"

_0)

10

10

10

^10"4

n-l
L"o

c
Z 10

"O

10
10

10

10

10
10

10
10

100

da/dN (10"6in/cycle)

I I I M

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

3.28
3.46
5.69
10.0
18.6
32.7
55.1
90.4
228.
405.

12.70 (min)
13.

16.
20.
25.
30.
35.
40.
50.
56.60 (max)

RMS %
Error
25.51

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i 11111

Life Prediction Ratio Summary

RMS %
Error

Life Prediction Ratio Summary

i--

0.

.5

.8

1.25

0.

2.

Figure 5.11.3.1.4
5-169

.5

.8

1.25

RENE 95 (H&F)
Condition/Ht: 2000F 1HR
Form: 1.23 in. Forging
Specimen Type: KB Bar
Orientation: CR
Stress Ratio: 0.05
Frequency: 0.3 Hz

SQ

Yield Strength: 171 ksi


Ult. Strength:
Specimen Thk: 0.25 in.
Specimen Width: 0.6 in.
Ref: GE001
(1 Of 1)

AK (MPaVin)
4

10

40
-l

Z=r-\i l i I i|i

AT 1000F

AK (MPaVin)
4

100

(=I

1 I I I llll

10

40

1 I I Mil

100

' I M'l'l

-Environment: Lab Air; 1200T 10


-2

10

10

10

10
10

10
JU
o

-Jio"2

6-10-4

i o"+

_c

_
10

10

10

-5

_^-o
10

10

10

10
10

10

10
10

10
4

10

40

da/dN (10-6in/cycle)

Life Prediction Ratio Summary


i

0.

40

100

da/dN (10~6in/cycle)

AK (KsiVin)

2.02
4.44
9.83
18.3
30.2
49.1
82.0
155.

13.58 (min)
16.
20.
25.
30.
35.
40.
45.70 (max)

RMS %
Error
16.78

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I I I I III

I I I I III

100

.5

.8

RMS %
Error

Life Prediction Ratio Summary


i

0.

1.25
Figure 5.12.3.1
5-170

.5

.8

1.25

]-

2.

WASPALOY

II
S*

3
-
J

S8
W

iS

OB

3
o
fa

5-171

-I WAS PALO Y h
Condition/Ht:
Form:
Specimen Type: CT
Orientation: C-R
Stress Ratio: 0.05
Frequency: 0.3 Hz

Yield Strength: 154 ksi


Ult. Strength: 199.2 ksi
Specimen Thk: 0.25 - 0.452 in.
Specimen Width:
Ref: PW006
(1 of 2)

AK (MPaVin)
4

10

- I ' I Tl'l

40

100

- I

' I 'I'l'l

(2 of 2)

AK (MPaVin)
10

' I 'I'l'l

40

100

' I 'I'l'l

Environment: Argon; 1200T

Environment: Lab Air; 1200F

-=d

-2

10

10

10

10

-3

10

10
_0J

10

10

SMcf

-Z. 10

"*"*

o
6-10-4

_0J

10

z: 10

"O

ior\
o

_A"0
10

T3

10

10

10

10

10

10

10

10
10

, I,I,I,
4

I , LI,I,

10

40

.-8

' i i nil
4
10

10

100

da/dN (10"6in/cycle)

RMS *
Error
1.73

i-'

.5

.8

1.25

100

18.2
21.9
29.8
35.3
42.8

33.32 (min)
35.
40.
50.
59.56 (max)

Life Prediction Ratio Summary


0.

i i iii

da/dN (10"6in/cycle)

AK (KsiVin)

5.71
6.28
9.44
15.3
22.6
29.8
31.0

14.91 (min)
16.
20.
25.
30.
35.
35.87 (max)

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'

2.

RMS %
Error
9.57

Figure 5.13.3.1.1
5-172

Life Prediction Ratio Summary


.5

.8

1.25

2.

WASPALOY
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CT
Orientation:
Stress Ratio: 0.05
Frequency: 20 Hz

Yield Strength: 154 ksi


Ult. Strength: 199.2 ksi
Specimen Thk: 0.753 in.
Specimen Width: 2.505 in.
Ref: PW001
(1 of 1)

AK (MPaVin)
1

10

40

AK (MPaVin)

100

4
_

10

| . |.|.|

40
|

100

| . jT|

Environment: Lab Air; 1200T 10

10

10
10

10

10

10

10" ^

_Q3

io'2^

5^10-4

o 10
\
c

-3 I

tr

2 10

10

..-o

_.L~a

10

10

10

10
10

D
TO

10
-7

10

10
10

" I , I,I,I,
4

10

I , I.LI,

10

40

10

100

AK (KsiVin)

30.41 (min)
35.
40.
44.85 (max)

RMS %
Error

40

100

da/dN (I0"6in/cycle)

AK (KsiVin)

11.0
13.7
18.8
29.4

Life Prediction Ratio Summary


i

0.

10

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

3.19

-Z. 10
-

10

j.

10

.5

.8

RMS %
Error

Life Prediction Ratio Summary

1.25

0.

Figure 5.13.3.1.2
5-173

.5

.8

1.25

\ WASPALOY I
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CT
Orientation: CR
Frequency:
Environment: LAB AIR;1200F
(1 of 1)

AK (MPcVin)
4

10
i

Yield Strength: 154 ksi


Ult. Strength: 199.2 ksi
Specimen Thk: 0.316 - 0.422 in.
Specimen Width: 2.504 - 2.509 in
Ref: PW001
AK (MPaVin)
4

40
100
I ' I il'l

- I

10

I 'I'l'l

40

100

' I M'l'l

10

-2

10

10

10

io"2^
o

-3 )=

10

Z 10
10
O
"O

-6

10

10
10

10
4

10

40

100

100

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycie)
16.2
22.3
54.9
103.
170.
394.
885.
2061.
5074.
7701.

23.65 (min)
25.
30.
35.
40.
50.
60.
70.
80.
84.43 (max)

RMS %
Error
38.52

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

Life Prediction Ratio Summary


on x
a,

0.

.5

.8

1.25

RMS %
Error

1""

2.

Figure 5.13.3.1.3
5-174

Life Prediction Ratio Summary


0.

.5

.8

1.25

uunnAi r\\/

K
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CT
Orientation: C-R
Frequency:
Environment: LAB AIR;1350F

(1 of 1)

AK (MPaVin)
4

10

40

-I'l 'I'l'l

Yield Strength: 154 ksi


Ult. Strength: 199.2 ksi
Specimen Thk: 0.299 - 0.3 in.
Specimen Width: 2.504 - 2.511 in.
Ref: PW001

' I UTI

_L

10

Stress Ratio: 0.1

ID"2

I'l' I'l'l

IQ"3

io"

(in/cyc

(in/cyc

-6

10

^E

z:

ZIG"5

10
-

\
D

\
o
"

10

QJ

o
\

-*?
10

>
O
~u

-6
10
-5

la"7

-6

10

I , LU

I , I -M,
10

_ 1 , 1,1,1,

in"8
1

1C)0

40

6
da/dN (10 " in/cycle)

11.82

Life Prediction Ratk5 Summary


no
i

0.

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

17 6
25 5
37 6
93 8
150.
150.

31.69 (min)
35.
40.
50.
60.
60.02 (max)

RMS %
Error

I , I,I,I,

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

E^

10

~^ 10

"

o
\

-3^

-5

IQ"7

<D

1jT&

10

10

,n-

10

-1
10

<D

ID

"C

100

10

Z10"5

-I'M I'l'l

40

-1

Q>

10

la"2

la"3

AK (MPaVin)
4

100

.5

.8

RMS %
Error

Life Prediction Ratio Summary

1.25

6.

2.

Figure 5..13.3.1.4
5-1 75

.5

.8

1.25

2.

] WAS PALO Y I
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CT
Orientation: CR
Frequency: 20 Hz
Environment: LAB AIR;1200F

Yield Strength: 154 ksi


Ult. Strength: 199.2 ksi
Specimen Thk: 0.3 - 0.302 in.
Specimen Width: 2.503 - 2.518 in
Ref: PW001
(1 of 2)

AK (MPaVin)
4

- I

10

40

' I 'I'l'l

100

-Ml

' I M'l'l

Stress Ratio: 0.1

10

40

M'l'l

100

' I M'l'l

_L

Stress Ratio: 0.8

10

10

10

u
u 10

O
+

fcl 0"
c

"

10

-3^

10

E
-5

10

2 10

2 10

io \
o

10

10

jd

-= 10

10

10

=:

~ 10

10

I , I,I,I,

" I , I,I,I,
4

10

40

10

~ I ,
4

100

da/dN (10'6 in/cycle)

0.

.5

.8

100

1.25

0.761
0.801
0.947
1.10
1.28
2.43

6.75 (min)
7.
8.
9.
10.
13.
14.64 (max)

40

da/dN (10"6in/cycle)

AK (KsiVin)

2.04
3.73
6.59
9.62
13.0
15.8

Life Prediction Ratio Summary


i

10

AK (KsiVin)

16.66 (min)
20.
25.
30.
35.
38.72 (max)

RMS %
Error
7.34

I , MM,

Mill

AK (KsiVin)
AK (KsiVin)

D
X>

~ 10

10

10

10

10

10

XJ

(2 of 2)

AK (MPaVin)

2.

RMS %
Error
7.28

Figure 5.13.3.1.5
5-176

3.92

Life Prediction Ratio Summary


CD
i

0.

.5

.8

1.25

2.

This page intentionally left blank

5-177

pH WASPALOY I
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CT
Orientation: C-R
Stress Ratio: 0.05
Frequency: 0.2 Hz

Yield Strength: 154 ksi


Ult. Strength: 199.2 ksi
Specimen Thk: 0.102 - 0.501 in.
Specimen Width: 2.486 - 2.519 in.
Ref: PW001

AK (MPaVin)
4

10

40

I ' I 'I'l'l

-)

10

(2

AK (MPaVin)

100

I ' I Tl'l

=
Environment: Lab Air; 800T

la"2

of 3)

10

40

io~2

-i

10

io"3

^-^

IG"3

<u
o

IQ'2

o
\

d
ME

Z^s

10

ZIG"

10

>
o

&
*'

10"6

JS#\sf
w

"'

ZIG"5

\
a

'

io"2
o
\

U-10-4

jfgm

10

io~7

ID'7

~~
-6

-6

10

10

"

I'

,' I'',l,l,

I'

,'
I , i ,l,

10

40

100

I , I,I,I,

" I , I,I,I,

io"8

10

40

100

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'
z

-5

-5

10

-8

vE

jf
f

10

10

""~*

1 U

3)

I ' I ' I'l'l


I ' I ' I'l'l
-1
0
Environment: Lab Air; 1200T 10

10

o
6^10"+
\
c

100

da/dN (lO^in/cycle)

17.25 (min)
20.
25.
30.
35.
40.
50.
58.47 (max)

da/dN (10"6in/cycle)

AK (KsiVin)
17.60 (min)
20.
25.
30.
35.
40.
50.
60.
70.
76.85 (max)

1.57
2.32
4.28
7.01
10.4
14.4
22.8
29.4

6.24
8.79
13.3
19.6
32.5
50.4
41.3
21.8
42.1
45.9

'

RMS %
Error
44.49

Life Prediction Ratio Summary


a
o
+A
i

0.

.5

.8

1.25

2.

RMS %
Error
5.85

Figure 5.13.3.1.6
5-178

Life Prediction Ratio Summary


a o
0.

.5

.8

1.25

2.

WASPALOY
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CT
Orientation: CR
Stress Ratio: 0.05
Frequency: 0.2 Hz

Yield Strength: 154 ksi


Ult. Strength: 199.2 ksi
Specimen Thk: 0.102 - 0.501 in.
Specimen Width: 2.486 - 2.519 in
Ref: PW001
(3 of 3)

AK (MPaVin)

AK (MPaVin)
4

4
10
40
100
_ I I I ljllll
I I 111>l'l
-1
Environment: Lab Air; 1350T 10

~
10

IQ"3
-2>
o

o 10
\
c
10
"u

_K

10

10

10

= I

.52
io"2^

-3 |
10 E

n^^^HS^

&F

-A.T>
10 o

-5
10

" I I,I,I,
4

I , I,hi,

10

40

C)

z:

10

10 \
-o

x>

_c 10
10
10
10

10
4

10

40

100

AK (KsiVin)

da/dN (10"6in/cycle)

da/dN (10*6in/cycle)

AK (KsiVin)

15.2
18.6
23.4
22.8
25.0
36.3
42.1

<o

10~ |

Life Prediction Ratio Summary


0.

o
o 10

100

23.76 (min)
25.
30.
35.
40.
50.
56.57 (max)

RMS %
Error
9.06

10

AK (KsiVin)
AK (KsiVin)

100

' I 'l'l'l

10
_Q3

10

40

10

10

' I 'I'l'l

.5

.8

1.25

2.

RMS %
Error

Life Prediction Ratio Summary


t

0.

.5

.8

Figure 5.13.3.1.6 (Concluded)


5-179

1.25

2.

\ WAS PALOY I
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CT
Orientation: C-R
Stress Ratio: 0.1
Frequency: 20 Hz

Yield Strength: 154 ksi


Ult. Strength: 199.2 ksi
Specimen Thk: 0.307 - 0.5 in.
Specimen Width: 2.508 - 2.51 in.
Ref: PW001
(1 of 2)

AK (MPaVin)
!=I

4
10
40
100
Ii i i i iiii
1 I l I l

Environment: Lab Air; 800T

(2 of 2)

AK (MPaVin)
10

- I ' I M'l'l

40

100

-1

I ' I TIN

Environment: Lab Air; 1200T 10

10
-2

10

10
10

-=

<o

10"
o

10

10

">'

U
6-10"4

10

o
6-10-4

10

10
10

T3

10"

z
-= 10 ^
u
x>

10

10

:
10

10

10

10
'

i I i I in
4
10

i iiHI
40

10

- i , i,i,i,
4

100

da/dN (10"6in/cycle)

AK (KsiVin)

13.3
19.9

.5

.8

40

100

1.25

da/dN (10"6in/cycle)
4.85
8.72
12.5
16.2
21.5
24.6

20.71 (min)
25.
30.
35.
40.
42.08 (max)

Life Prediction Ratio Summary


0.

10

AK (KsiVin)

2.96
4.45
6.72
9.60

20.94 (min)
25.
30.
35.
40.
46.62 (max)

i , i,i,i,

AK (KsiVin)

AK (KsiVin)

RMS %
Error
5.34

^-^

10

10

10

'1

2.

RMS %
Error
11.97

Figure 5.13.3.1.7
5-180

Life Prediction Ratio Summary


0.

.5

.8

1.25

-H WAS PALOY
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CT
Orientation: CR
Stress Ratio: 0.05
Environment: LAB AIR;1200F

10

Yield Strength: 154 ksi


Ult. Strength: 199.2 ksi
Specimen Thk: 0.432 - 0.447 in.
Specimen Width: 2.502 - 2.503 in
Ref: PW001
(1 of 2)

AK (MPaVin)
' I M'l'l

(2 of 2)

AK (MPaVin)
1

40
100
-ii I i I Mil

b I
10

Frequency: 0.33 Hz

10

40

' I 'I'l'l

100

' I M'l'l

=1

Frequency: 20. Hz

10

10
10

10
10"2

o
o 10

-o

10" |

:z 10

2
10"
o

_
10

,-s
10

10

10

10

_QJ

_Jio \

z
fz

m" ^
u
XJ

"O

T3

10

10

10

10
10

10

10

10
' i i i in
4
10

10

I I i I Hi
40
100

I I iI Mi
4
10

10

da/dN (10"6in/cycle)

176.
309.

76.26 (max)

RMS %
Error
7.02

Life Prediction Ratio Summary

0.

.5

.8

da/dN (10"6in/cycle)

AK (KsiVin)

4.06
4.32
7.45
11.0
14.8
21.1
23.9

18.78 (min)
20.
25.
30.
35.
40.
42.53 (max)

18.3
19.6
26.2
32.8
54.9
74.3

29.22 (min)
30.
35.
40.
50.
60.
70.

i 11 li
100

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

40

1.25

2.

RMS %
Error
2.80

Figure 5.13.3.1.8
5-181

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

^ WAS PALOY I
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CT
Orientation: CR
Stress Ratio: 0.1
Environment: LAB AIR;1200F
(1 of 1)

AK (MPaVin)
1

10

i i 'i'l'l

Yield Strength: 154 ksi


Ult. Strength: 199.2 ksi
Specimen Thk: 0.318 in.
Specimen Width: 2.484 in.
Ref: PW001

40

AK (MPaVin)
1

100

Ir ' I 'I'l'l

Frequency: 0.17 Hz

10

-Ml 'I'l'l

40

100

' I 'I'l'l

10
10

10

10

10

10

-2

10

io

10"
o
6^10-4

10"

Z 10
a

10
10

"O

10
10

10

10

10

10

10

10

i l i 111

i I il in

10

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


,

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

7.03
10.4
17.1
25.1
33.6
41.5
44.6

16.71 (min)
20.
25.
30.
35.
40.
42.17 (max)

0.

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
8.10

''

-z.

10

10

=1

*"o
4
in \
u

tn

XI

T7

-3 |

10

<0
V

.5

.8

1.25

2.

RMS %
Error

Life Prediction Ratio Summary


i

0.

Figure 5.13.3.1.9
5-182

.5

.8

1.25

_l
I

Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CCP (max load specifie d)
Orientation:
Frequency: 0.2 Hz
Environment: LAB AIR;1200F

AK (MPaVin)
4

1
_

10

40

i | i|i|i|

of 2)

10

Stress Ratio: 0.1

io~
o

<o
u
u 10

10

Jr

(B^
2r

Z10"5
o

\
o
~

&
r?

-6
10

~
10 \
o
XI

-1

__
a>
io~2

10 E
z:

-1

J?

X)

cF

10 >
o

o
,-
10

X
-5

-5

10
-

io-7

-6

-6

" I , LI,I,

m"8
1

I , I,I,I,

10

40

- 10
-

10
m"8

- 1 , 1,1,1,
1

100

da/dN (10"6in/cycle)

11.83 (min)
13.
16.
20.
25.
30.
35.
40.
50.
51.07 (max)

RMS %
Error
13.74

E>
i

10

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

2.34
3.35
6.64
12.1
20.4
30.6
43.4
60.0
111.
119.

Life Prediction Ratio Summary


0.

I , I,I,I,

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

Z10"5

10
-

io"7

_i
10

io"3

<U

o 10

40
100
i | jijij

10

0)

4
10
i | i |i|i|

Stress Ratio: 0.55

-1

ID"3

10~2

10~2

(2 of 2)

AK (MPaVin)
1

-L

I p

Yield Strength: 154 ksi


Ult. Strength: 199.2 ksi
Specimen Thk: 0.287 - 0.297 in.
Specimen Width: 0.973 - 0.998 in.
Ref: PW001

100

' | i|'|i|

\A/Aor>Ai rv
VVttorMLU I

.5

.8

1.25

2.

RMS %
Error

Life Prediction Ratio Summary


0.

Figure 5.13.3.1.10
5-183

.5

.8

1.25

2.

^ WASPALOY I
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CCP (max load specified)
Orientation:
Stress Ratio: -1
Frequency: 0.2 Hz
(1 of 2)

AK (MPaVin)
1

4
10
t=II I ' I MM

Yield Strength: 154 ksi


Ult. Strength: 199.2 ksi
Specimen Thk: 0.297 - 0.3 in.
Specimen Width: 0.997 in.
Ref: PW001

40
100
1I I I MI'I

Environment: Lab Air; 800F

(2 of 2)

AK (MPaVin)
|

10

40

l|l|l|

100
.,.,,,

-2

10

10

10

"^

10
10

5M O"

10
D

10

10
10
10
10
i

10

111111

10

10

D
" -6
10

10

-8

iF

JF
6

da/dN (10"6in/cycle)

37.90 (max)

0.

.5

.8

100

1.25

2.32
3.84
6.44
10.5

11.63 (min)

13.
16.
20.
25.
30.
31.47 (max)

Life Prediction Ratio Summary


1

40

da/dN (10"6 in/cycle)

AK (KsiVin)

1.74
2.18
4.80
9.05
13.7
23.6
32.6

10

AK (KsiVin)

35.

1 , 1,1,1,

i 1 i 1111

100

15.16 (min)
16.
20.
25.
30.

RMS %
Error
6.56

10" N
'
z

m" ^
u
XJ

10
-6

AK (KsiVin)
AK (KsiVin)

10

<

o
10~
"^
o

o
u 10
\
c

10

1111 n

40

-X

Environment: Lab Air; 1200T 10

10

2.

RMS %
Error
3.61

Figure 5.13.3.1.11
5-184

17.3
25.8
23.4

Life Prediction Ratio Summary

0.

.5

.8

1.25

2.

J
i
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CCP (max load specifie d)
Orientation:
Stress Ratio: -0.5
Frequency: 0.2 Hz

(1

AK (MPaVin)
1

10

40

io-2

ID"3

= I

Z10"5

\
a

-1

io"3

frio"4

_3E
io E

_c

XI

\
o
10
-6

10

-5

10

10

10"7

-6

-I

10

i , Lhi,
4

I , I.I.L

10

40

_ I , I,I,I,

10"8
1

100

da/dN (10~6in/cycle)

16.44 (min)
20.
25.
30.
31.61 (max)

.8

100

da/dN (10"6in/cycle)

RMS 55

7.33
9.57
11.4
18.7

Life Prediction Ratio Summary

Error

- iii

.5

40

17.29 (min)
20.
25.
27.24 (max)

0.

10

AK (KsiVin)

1.39
5.75
8.69
16.7
16.2

Life Prediction Ratio Summary


i -

I , I, I,I,

-6

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

>
o
X

-5

9.89

-z.

tP

XI

m
UJ

-6
10

Q>

io"2

03
U

2 10-5

10 \
o

sff

Ml

10

jSM

T3

RMS %
Error

' I 'l'l'l

10

o
^10"4
_c

100

io"2

io"2
J
o

3 E
10"3E

m"8

' I ' I'M

40

Environment: Lab Air; 1200T 10

CD

10~7

10

-1

to

"

(2 of 2)

AK (MPaVin)
1

100

Environment: Lab Air; 800F

iI ^

Yield Strength: 154 ksi


Ult. Strength: 199.2 ksi
Specimen Thk: 0.298 in.
Specimen Width: 0.996 - 0.998 in.
Ref: PW001

of 2)

10

\A/ACHA
vv/-\or/-\ l(Tv

1.25

9.50

2.

Figure 5.13.3.1.12
5-185

0.

.5

.8

1.25

2.

i WAS PALOY I
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CCP (max load specified)
Orientation:
Stress Ratio: 0.05
Frequency: 0.2 Hz

Yield Strength: 154 ksi


Ult. Strength: 199.2 ksi
Specimen Thk: 0.301 - 0.303 in.
Specimen Width: 0.996 - 0.998 in
Ref: PW001

(1 of 3)

AK (MPaVin)

(2 of 3)

AK (MPaVin)

4
10
40
100
i I i HIM
1i I i MIM
- Environment: Lab Air; 1200F 10

4
10
40
100
-1
1 I I I llll
pr-Ti I i I IM
- Environment: Lab Air; 800F 10
10

10

10

10
10

10

_0)

-J10"

o
frlCf4

o
o^10'4

-3 |

-3^

10

10

10

10
T3

XI

10

XI

10

X)

.-6

XI

o
x>

10

10

-5

10

10

10

10

10

10
'

10

i i i n

10

40

' 11

10

i i ii ii

100

da/dN (I0"6in/cycle)

AK (KsiVin)

41.48 (max)

.5

.8

40

100

10.8
14.1
19.8
30.3
44.7
58.1

43.07 (max)

1.25

da/dN (10"6in/cycle)

23.34 (min)
25.
30.
35.
40.

Life Prediction Ratio Summary

0.

10

AK (KsiVin)

3.81
5.56
8.66
13.7
23.2
27.5

21.55 (min)

25.
30.
35.
40.

LI

i i i im

II

AK (KsiVin)

AK (KsiVin)

RMS %
Error
1.89

2.

RMS %
Error
1.81

Figure 5.13.3.1.13
5-186

Life Prediction Ratio Summary


a
i

0.

.5

.8

1.25

2.

_l

U/APnA

Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CCP (max load specified)
Orientation:
Stress Ratio: 0.05
Frequency: 0.2 Hz

- I

10

' I 'I'l'l

40

4
_

10

| i|i|i|

40
|

1 r

100
|i|i|

Environment: Lab Air; 1350T 10

j.

10

10~2

10"2

-1

10

ID"3 _

\
_c

~Z- 10

io"
o

6"10-4

\
D

-5

~Z. 10

\
o
"

XI

-6
10

_c

*~
10 \

XI

V
2
io"

-3p
10 E,

<D

-3P
10 E

-i

10

la"3

a>
2

a;
o
o 10

AK (MPaVin)
1

100

' I 'I'l'l

L0

Yield Strength: 154 ksi


Ult. Strength: 199.2 ksi
Specimen Thk: 0.301 - 0.303 in.
Specimen Width: 0.996 - 0.998 in.
Ref: PW001

(3 of 3)

AK (MPaVin)
4

VVMOTM

-z.
-4.P
__ 10 >
o
XI
_

-6

10

-5

-5

10

10"7

10

10"7

-6

-6

" I , I, I,I,

m"8
1

10

Mill

40

10
-

" 1 , 1,1,1,

m"6
1

100

RMS %
Error

da/dN (10"6in/cycle)

Life Prediction Ratio Summary


i

0.

1-

.5

.8

40

100

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , I,I,I,

10

10
-

1.25

da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error

Life Prediction Ratio Summary

0.

2.

Figure 5.13.3.1.13 (Concluded)


5-187

.5

.8

1.25

2.

-I WAS PALOY I
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CCP (max load specified)
Orientation:
Stress Ratio: 0.5
Frequency: 0.2 Hz
(1 of 1)

AK (MPaVin)
4
c=Ii

10

I i I i|>

Yield Strength: 154 ksi


Ult. Strength: 199.2 ksi
Specimen Thk: 0.3 in.
Specimen Width: 0.995 in.
Ref: PW001
AK (MPaVin)
4

40
100
1I I M 'IM

- Environment: Lab Air; 800T

10

40

100

- I ' I 'I'l'lI ' I Tl'l3


10

10

10
-1

10
-3

10

10
o
o 10

o
c^10-4

10

10
10

o
\

3E

-z.

Z 10

4t. "n

"O

in \
u
-o

XI

10

10

10

10

10

10

10

10

10

1 I III

10

10

I I I 111

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

40

100

da/dN (10_6in/cycle)

AK (KsiVin)

3.88
3.92
5.91
10.4
14.6

15.92 (min)
16.
20.
25.
28.39 (max)

Life Prediction Ratio Summary

RMS %
Error

Life Prediction Ratio Summary


i

0.

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
1.98

10~

E
a

QJ

10"

.5

.8

0.

1.25

Figure 5.13.3.1.14
5-188

1i

.5

.8

1.25

2.

WASPALOY
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CCP (max load specified)
Orientation:
Stress Ratio: 0.8
Frequency: 0.2 Hz
(1 of 2)

AK (MPaVin)
4
I

10

I i I MM

40
T

Yield Strength: 154 ksi


Ult. Strength: 199.2 ksi
Specimen Thk: 0.3 in.
Specimen Width: 0.996
Ref: PW001

100

Environment: Lab Air; 800F

(2 of 2)

AK (MPaVin)
prii

I II MM

10

40

i i 1111

1I

100

I I I MM

Environment: Lab Air; 1200T 10

10
10

10

10

10
10

10
2

10"
O

o 10

io"2

o
o 10

,o4

-3 |

10

Z10

|-

T3

10
"O

0.998 in.

XI

_c -

10
10

"O

_K

10

10

10

10
10

10

10

10
10

I i I Hi

10

10

I iI Hi

40

da/dN (10~6in/cycle)

RMS %
Error
21.44

0.

.5

1-

.8

100

1.25

0.861

5.59 (min)
6.
7.
8.
9.
10.
11.87 (max)

Life Prediction Ratio Summary


T

I iI Mi

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.434
0.765
0.791

6.02 (min)
7.
7.32 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I i 1111

100

2.

RMS %
Error
4.25

Figure 5.13.3.1.15
5-189

1.42
2.00
2.60
3.36
3.90
5.76

Life Prediction Ratio Summary

0.

.5

.8

1.25

2.

H WAS PALO Y I
Condition/Ht:
Form: 1.6 in. Forging
Specimen Type: CCP (max load specified)
Orientation: CR
Stress Ratio: 0.1
Frequency: 0. Hz
(1 of 1)

AK (MPaVin)
4
-

10

| l|l|>|

40
|

'

Yield Strength: 154 ksi


Ult. Strength: 199.2 ksi
Specimen Thk: 0.299 in.
Specimen Width: 0.998 in.
Ref: PW001

AK (MPaVin)
4

100

| 'l'l'l

10

-Ml 'I'l'l

-L

40

100

' I M'l'l

10

Environment: Lab Air; 1200T 10


-2

10

10

10

10

-3

10

10

"*"*

io"

.5?

6^10-+

io"2

10

o^10"4

10

-Z. 10

z: io

10'\
O

XI

TJ

\
o

_xX

10
_, h-

XJ

o
x>

10

10
-5

10

-= 10

10

10

10

-= 10

10

"

I , I,I,I,

I , I,I,I,

40

10

10
4

100

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary

100

da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error

Life Prediction Ratio Summary


i

0.

40

12.5
22.2
30.0
44.3
75.4
109.

21.41 (min)
25.
30.
35.
40.
45.95 (max)

RMS %
Error
5.56

10

AK (KsiVin)

AK (KsiVin)

.5

.8

1.25

.5

2.

Figure 5.13.3.1.16
5-190

.8

1.25

WASPALOY
Condition/Ht: 1850F 2HRS
Form: 1.18 in. Billet
Specimen Type: CT
Orientation:
Stress Ratio: 0.1
Frequency: 10 Hz

1350F 6HRS
Yield Strength: 145 ksi
Ult. Strength: 249 ksi
Specimen Thk: 0.125 in.
Specimen Width: 1.25 in.
Ref: UC001
(1 of 1)

AK (MPaVin)
4
10
f=ii I i Ml'

FT

40
100
-ii I i I MM

AK (MPaVin)
1

=q

4
10
rrIi I i I MM

40
I

100

I I I MM

10

10

Environment: Lab Air; R.T.


-2

10

10

-2
10

10
-3

10

10

JO

io"2
o
o 10

x>

u 10

10

10
10

10

10

-5

o
10

10

10

10
10

10

10

10
10

i l i 11 li
40
100

i l i l in
4
10

10

'

da/dN (I0"6in/cycle)

Life Prediction Ratio Summary


0.

40

100

da/dN (I0"6in/cycle)

AK (KsiVin)

1.09
1.38
2.75
4.57
10.5
14.7

27.75 (min)
30.
35.
40.
50.
53.11 (max)

RMS %
Error
2.44

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I I I I III

I i I i li

.5

.8

RMS %
Error

Life Prediction Ratio Summary

0.

1.25

Figure 5.13.3.1.17
5-191

.5

.8

1.25

\ WAS PALO Y I
Condition/Ht: 1850F 2HRS
Form: 1.18 in. Billet
Specimen Type: CT
Orientation:
Stress Ratio: 0.1
Frequency: 10 Hz

1600F 24HRS (FINE GS


Yield Strength: 111.5 ksi
Ult. Strength: 228 ksi
Specimen Thk: 0.125 in.
Specimen Width: 1.25 in.
Ref: UC001
(1 of 1)

AK (MPaVin)
4

B I

10

' I M'l'l

40

AK (MPaVin)
4

100
1

' I 'l'l'l

r I

M 'I'l'l .

40

100

' I Tl'l

10

Environment: Lab Air; R.T.

10

10

10

10

10

10

10

<D

_a;
o

10

-3|
10
E

jo
o

io"2

^1

5^10-

3*10"
c

10

10

T>

10

10

"D
10

-o

10

10
-5

10

10
-J

10

10

10

_e

" 1 , 1,1,1,
4

10

10

1 , 1,1,1,

10

40

10
4

100

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)

40

Life Prediction Ratio Summary

da/dN (10_6in/cycle)

AK (KsiVin)

RMS %
Error

Life Prediction Ratio Summary


ii

0.

100

1.03
2.33
4.39
7.13
10.9

25.47 (min)
30.
35.
40.
45.09 (max)

RMS %
Error
2.60

10

AK (KsiVin)

.5

.8

.5

1.25

Figure 5.13.3.1.18
5-192

.8

1.25

This page intentionally left blank

5-193

\ WASPALOY I
Condition/Ht: 1875F 4HRS OQ
Form: Disk
Specimen Type: WOL
Orientation: CR
Stress Ratio: 0.05
Environment: LAB AIR;1200F

(1 of 3)

AK (MPaVin)
4
10
r-rrpir

1550F 4HRS AC
Yield Strength: 153.7 ksi
Ult. Strength: 199.7 ksi
Specimen Thk: 0.5 in.
Specimen Width: 2.5 in.
Ref: PW004
(2 of 3)

AK (MPaVin)
1

40
100
i I i I mi

40
100
-ii ! i mil=n
.
10
Frequency: 0.33 Hz

= I

Frequency: Unspecified

10

' I'l'l'l

-2

10

10
la"3

io"2

o
6^10-4

-3 ?=

10

10
10

10
10
10
10
10
4

10

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error
49.61

0.

.5

.8

100

1.25

1.94
2.84
5.27
8.42
12.3
17.0
23.5
31.7
47.3
59.0
97.1
222.
360.

11.78 (min)
13.
16.
20.
25.
30.
35.
40.
50.
60.
70.
80.
89.65 (max)

Life Prediction Ratio Summary


i

40

da/dN (10"6in/cycle)

AK (KsiVin)

15.2
16.7
38.2
77.1
140.
360.
745.
1443.
2886.
7179.
13261.

24.46 (min)
25.
30.
35.
40.
50.
60.
70.
80.
90.
95.27 (max)

10

AK (KsiVin)

AK (KsiVin)

I-'

RMS %
Error

20.49

2.

Figure 5.13.3.1.19
5-194

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

H WASPALOY

(3 of 3)

AK (MPaVin)
1

b I

10

40

' I 'I'l'l

AK (MPaVin)
4

100

' I M'l'l

Frequency: 20 Hz

|=I

10

I I Mil

40
100
1I I I MM

10

10
10

10

10

10
10

ID"3
2

-Jio"
o

o
^10"+

io"2

-S2
o

6^10-*
3

10" E

10

-5

-5

10

10

.i.tj
-4,

10

x>

1550F 4HRS AC
Yield Strength: 153.7 ksi
Ult. Strength: 199.7 ksi
Specimen Thk: 0.5 in.
Specimen Width: 2.5 in.
Ref: PW004

Condition/Ht: 1875F 4HRS OQ


Form: Disk
Specimen Type: WOL
Orientation: C-R
Stress Ratio: 0.05
Environment: LAB AIR;1200F

_.
10

o
-a

-Jio \
-o

"O

10

-5

10

10
-7

10

10

10

10
.-8

10

10

-8

. I.I.I.
40

10

LL

da/dN (10_6in/cycle)

Life Prediction Ratio Summary

100

da/dN (10~6in/cycle)

AK (KsiVin)

.5

RMS %
Error

Life Prediction Ratio Summary


i

r-

0.

40

3.55
3.86
6.37
9.75
13.9
18.8
29.7
30.2

19.24 (min)
20.
25.
30.
35.
40.
50.
50.41 (max)

RMS %
Error
14.62

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

. i. iin

I i I Hi

100

.8

0.

1.25

Figure 5.13.3.1.19 (Concluded)


5-195

i-

r-

.5 .8

1.25

2.

WASPALOY
Condition/Ht: 201 OF 2HRS
Form: 1.18 in. Billet
Specimen Type: CT
Orientation:
Stress Ratio: 0.1
Frequency: 10 Hz

1350F 6HRS
Yield Strength: 95 ksi
Ult. Strength: 230.5 ksi
Specimen Thk: 0.125 in.
Specimen Width: 1.25 in.
Ref: UC001
(1 of 1)

AK (MPaVin)

AK (MPaVin)
4

4
10
40
100
-II I 11 till
f=-lI I i MP
Environment: Lab Air; R.T.
-= 10

- I

-2

10

' I 'I'l'l

40

100

' I 'l'l'l

10

10

10

10
-3

-3

10

10

10"2
O
4

6^10-

o
6^10-4

,o-I

10

TJ

10

10

- 10 \
o
"o

_R
10

10

10
10

10

10

10
I

I I I I 11

10

10

I 11 III

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

1.16
2.80
11.0
22.0
24.0

43.83 (min)
50.
60.
70.
70.45 (max)

Life Prediction Ratio Summary


0.

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
12.70

10

10
T3

10

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


0.

2.

Figure 5.13.3.1.20
5-196

i-'

.5

.8

1.25

2.

WASPALOY
Condition/Ht: 201 OF 2HRS
Form: 1.18 in. Billet
Specimen Type: CT
Orientation:
Stress Ratio: 0.1
Frequency: 10 Hz

1600F 24HRS
Yield Strength: 96.5 ksi
Ult. Strength: 227.5 ksi
Specimen Thk: 0.125 in.
Specimen Width: 1.25 in.
Ref: UC001
(1 of 1)

AK (MPaVin)

AK (MPaVin)
4
10
t=ii I i n IT

4
10
40
100
i I i I MM
1i I <(!>!
Environment: Lab Air; R.T.
10

40
I

100

I 11 MM

10

10

10

10

10

10

_0)

u
10

10

10
o
6^10-4

\
10

E
10

10

-=ho \

-J10 >
10

10

10

10
10

10
10
10

ILLL
4

10

11 III

10

40

100

10

10

I I I III

40

100

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

'

I I I III

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

0.827
1.72
3.15
9.56
24.6

30.90 (min)
35.
40.
50.
59.23 (max)

RMS %
Error
2.82

Life Prediction Ratio Summary


i

.5

.8

RMS %
Error

1.25

Life Prediction Ratio Summary


0.

2.

Figure 5.13.3.1.21
5-197

.5

.8

1.25

TABLE 5.14

REFERENCES FOR THE NICKEL BASE ALLOY DATA

60578

INCONEL 718

K,

Christian, J. L., Yang, C. T., and Witzell, W. E., "Physical and Mechanical Properties
of Pressure Vessel Materials for Application in a Cryogenic Environment,"
ASD-TDR-62-258, Part III, General Dynamics/Astronautics (December 1964).
88187

INCONEL 718

K*

"Inconel 718 Test Data of September 19, 1973," Schultz Steel Company, South Gate,
CA., September 1, 1973.
88579

INCONEL 718

a-vs-N; da/dN

"B-l Program da/dN Data for Aluminum Alloys," Rockwell International Corporation:
Memorandum to H. D. Moran from E. W. Cawthorne, Battelle's Columbus
Laboratories, April 3, 1974.
88700

INCONEL 718

K^

Gilbreath, W. P., and Adamson, M. J., "The Stress Corrosion Susceptibility of Several
Alloys in Hydrazine Fuels," NASA Technical Note, Report NASA TN D-7604,
Ames Research Center, Moffett Field, CA, February 1974.
GE001

INCONEL 718
P/M RENE 95
RENE 95 (H&F)

da/dN
da/dN
da/dN

Shanini, V. and Popp, H. G., "Evaluation of Cyclic Behavior of Aircraft Turbine Disk
Alloys," General Electric, Evendale, Ohio, Contract No. NAS3-20368,
Report No. NASA-CR-159433, June 1978.
GE004

P/M RENE 95

a-vs-N; da/dN

"Argon Environment Testing," Thermal-Mechanical Crack Propagation Program; Data


Sheets sent from M. S. Gilbert, General Electric Co., Evendale, Ohio,
Contract No. F33615-77-C-5193, November 1980.
GE005

INCONEL 718

da/dN

"Fatigue Crack Growth Rate Data on Inconel 718 Using K Bar Specimens from the
TF34 DTA Effort;" Data sent from M. S. Gilbert, General Electric Co., Evendale, Ohio,
October 1982.

5-198

TABLE 5.14 (CONTINUED)


REFERENCES FOR THE NICKEL BASE ALLOY DATA

GE008

INCONEL 718
P/M RENE 95

da/dN
da/dN

Domas, P. A., "Crack Propagation Under Thermal Mechanical Cycling," General


Electric Co., Aircraft Engine Group, Evendale, Ohio, Contract No. F33615-77-C-5193,
November 1979.
HD003

INCONEL 600

a-vs-N; da/dN

James, L. A, "Fatigue Crack Propagation Behavior of Inconel 600," International


Journal of Pressure Vessels and Piping, Vol. 5, 241-259. 1977.
HD005

INCONEL 625

a-vs-N; da/dN

James, L. A, "The Effect of Temperature upon the Fatigue Crack Propagation


Behavior of Inconel 625," Report HEDL-TME 77-2, Westinghouse Hanford Co.,
Richland, WA, March 1977.
HD015

INCONEL 718

a-vs-N; da/dN

James, L. A, "Fatigue Crack Propagation Behavior of Inconel 718," Report HEDL-TME


75-80, Westinghouse Hanford Co., Richland, WA, September 1975.
HD016

INCONEL 718

a-vs-N; da/dN

Mills, W. J., and James, L. A, "Effect of Heat Treatment on Elevated Temperatures


Fatigue-Crack Growth Behavior of Two -Heats of Alloy 718," ASME Paper
78-WA/FVP-2, December 1978.
HD017

INCONEL 718

a-vs-N; da/dN

James, L. A, "The Effect of Product Form Upon the Fatigue-Crack Growth Behavior
in Alloy 718," Journal of Engineering Materials and Technology, Vol. 103, 234-239,
1981.
PW001

WASPALOY

a-vs-N; da/dN

Larsen, J. M., Schwartz, B. J., Annis, C. G Jr., "Cummulative Damage Fracture


Mechanics Under Engine Spectra," Pratt and Whitney Aircraft Group,
Government Product Division, West Palm Beach, Fla., Report No. AFML-TR-77-4159,
January 1980.

5-199

TABLE 5.14 (CONCLUDED)


REFERENCES FOR THE NICKEL BASE ALLOY DATA

PW002

IN100

a-vs-N; da/dN

Beyer, J. R., Sims, D. L., and Wallace, R. M., "Titanium Damage Tolerant Design Data
for Propulsion Systems," United Technologies Corp., Pratt and Whitney Aircraft Group,
West Palm Beach, FL, Report AFML-TR-77-101, Contract No. F33615-75-C-5130,
June 1977.

PW003

ASTROLOY 901
IN100
INCOLOY 901

da/dN
da/dN
da/dN

Fatigue Crack Growth Rate Data on Titanium and Nickel Base Alloys from B. S.
Schwartz, Pratt and Whitney Aircraft Group, Government Product Division,
West Palm Beach, FL., July 1982.
PW004

ASTROLOY P/M-H
ASTROLOY P/M-W
IN100 P/M-G
NASA IIB-7 P/M
WASPALOY

da/dN
da/dN
da/dN
da/dN
da/dN

Cowles, B. A., Sims, D. L., Warren, J. R., "Evaluation of the Cyclic Behavior of Aircraft
Turbine Disk Alloys," Pratt and Whitney Aircraft Group, United Technologies Corp.,
West Palm Beach, FL, Contract No. NAS3-20367, Report No. NASA CR-159409,
October 1978.
PW006

IN100
WASPALOY

a-vs-N; da/dN
da/dN

Fatigue Crack Growth Rate Data on Nickel Base Alioys from Pratt and Whitney
Aircraft Group, Government Product Division, West Palm Beach, FL., July 1982.

RI006

INCONEL 718

Kfae

Ferguson, R. R., Berryman, R. C, "Fracture Mechanics Evaluation of B-l Materials,"


Rockwell International B-l Division, Los Angeles, CA., Contract No. F33657-70-C-0800,
Report No. AFML-TR-76-137, October 1976.

UC001

WASPALOY

da/dN

Lawless, B., et al., "The Effect of Microstructure on the FCP and Overload Behavior
of Waspaloy at Room Temperature," Dept. of Materials Science and Metallurgical
Engineering, University of Cincinnati, December 1980.

5-200

CHAPTER 6
TITANIUM ALLOYS SECTIONS
6.0
6.0.1
6.0.2
6.0.3.1
6.0.3.2
6.0.4
6.0.5
6.1
6.2
6.3
6.4
6.5
6.6
6.7
6.8
6.9
6.10
6.11
6.12
6.13
6.14
6.15
6.16
6.17
6.18
6.19
6.20
6.21
6.22
6.23
6.24
6.25

Titanium Alloys Material Summaries


Available Data
Kie Summary
K Summary (Buckling not Constrained)
Ke Summary (Buckling Constrained)
FCGR at Defined AK Levels
Kfa Summary
BETA
BETAC
BETA m
BETATi
CORONA 5
EVH-834
Ti-*
Ti-10-2-3
Ti-4Al-3Mo-lV
Ti-5-2.5ELI
Ti-5Al-2.5Sn
Ti-6-2-2-2-2
Ti-6-2-4-2
Ti-6-2-4-2 ELI
Ti-6-2-4-6
Ti-6A1-4V
Ti-6A1-4VELI
Ti-6Al-6V-2Sn
Ti-6Al-6V-2.5Sn
Ti-6A12Sn4Zr6Mo
Ti-8Al-lMo-lV
Ti-Mo8V2Fe3Al
Ti-5A12.5Sn ELI
Ti-6A16V2Sn ELI
Titanium Alloys References

6-1

6-3
6-3
6-15
6-18
6-19
6-20
6-35
6-38
6-39
6-47
6-59
6-61
6-62
6-68
6-69
6-72
6-73
6-102
6-126
6-134
6-141
6-154
6-169
6-433
6-473
6-515
6-516
6-518
6-567
6-569
6-571
6-573

8
to

to

c-

CO

1-4

~C5

o
CO

CO

CO

Product
Form

-C

CJ
BJ

V
a

CD

53

55

53

35

35

C
o

a
a>
c

1a.

53

Ed

to
c
3

vV

u
V
c

I 1
CO
C
3

a
D

55

5
JS
cu

Condition/
Heat Treatment

ia
a
z
o

<

2^
O

o
o
CN

8
b.
o
c>
o
o

u.
o

8>o
lO

53
b.
o
CN

<
<

b.
io
*w

o
o

Ol

b.
o
o

u.
o
m
CN

b.
o
o

D
U
O

c
u
u

55

CN

b.
lO

lO

to

b.
o
CN
eo

d
b.
o
lO
co

<

55

b.
o

b.
o

or

&

35

<

o
o

<

b.
in

a
a
a

<+
<

C
CO
iO
CN
CO

EVI

Ed
CQ

to

eo

w
j _
gu
N
o
S
t q
*r Cu
o Sj

u.

o
C4
CQ

<:
VI

>>

M
a

<

6-3

i
CD

V
ir

I Is

3
J2
cu

es

Po

%
u

a ~
a
u
00 z

8
u,

h, O
i SI

o
a
z
u.

CO

CQ

tt

13
'S

>
S

p
rf

O
tf
o
CD

"8
s.

o o

&

c
D

a<:
<

a
2 -S
5
fl H

o 4
U 03

<

cs

o
u

s
o

<
U
a

z
<
oJ
a
u

<

<
OS

c
8.

BS

o
fror
o

>

s
CO

o
u

6-4

-3

as

2
Z

Z
U
P3 w

<
ES

3u
<

OJ

01

CN

M
-w

13

T3

os

01

13

04

e-

e-

T3
V
>
h
3

g
u

w
EH

o
O

CN

^"

CN

fa

co

o o
u fa

2
u

he

rf

es

be

C
o

bo

bo

'El

'S)

'Si

rf

rS

rS

o
a

be
'Si

<D
as

<

to

bo
B

o
o

be

fa

*>

2
O
O

<

OS
X

b.

b,

S3

S
P3

&

fa
o
o

fa

fa
s

63

Con diti on/


HeatT rea tmen

o
es

tf

<

Cd

a
a
o
o p
- O

o
to

<

as

CO

b.
o

<
os

b.
o
o
o

as

or

<
CD

b.

b.

b.

<

<
C5

EL.

O
LO
CN

b.
o
K

53

fao
fao
o

b.

o
os
B
EN
Ct,
o
o
o

fa
o

u
b.
OS

5
fa

53

OS

s
OS

o
Eu

fa

fa
S

fa
a

fa

s
s

fa

<
fa

8
en

>>
<
CD 5
O
Pi

6-5

fa
g

<

n
a

8u
7.
O

CN

fa

CO

CN

fa
s

fa

fa
S
c-

lO

<
OS

b.

Ia

en

CO

OS
K
CN

fa
s

<

3
OS

s
b.

cr

o
o

OS

b.

CO
CD

so

Of

(A

1
i

ifa
fa

00

OS
B
b.

oso
s <

EC
S

<
s

03

IS

s
to

b.

0}

b.

to

Of

fa
o
or

Cd
J
O
O

8
b.

CO

b.
&o
tCD

o
+

ff

<

5
to

fa

Of
03
OS
B
b.

S
as

CO

"'

tt

'S

13

T3

CO

13

OJ

CN

CN

t>

Ol

a
>

ti

rf

(N

00

10

CO

bo
E

C4

CO

o
CO

Produc
Form

-w

dition/
reatment

Ed
O

es
O
Eh

bo

&

bo

'Si

CO

bo
c

'S

.22

13

Ed

bo
C

&u

&

S.

CO
a

1
&
i

Ed

Cd

g
<

<

Ed Eh

a.

<H

OS

Ed
U

a
Ed
a
a
o

ca

<

Ch

a
es
o

Ed

Eh

2
2:

<

Ed

a
a
o

Eh

go

<

<
3

Ed

z
z<

<

<
5
OS

<

as
X

CO

CO
Eh
to
c*
co

a:

5
Eh

g
M

(N

CO
ES
CO

&.

<

eo

Ed

o
a

2.
-5

<

to

<

<

S
9
EQ
O

<

>

>

3 o

6-6

S3
<

CO

a
Ed
U

3
<

a
Cd
a

z-

Cd

63
5

CO

<

8
CO

s@

I i

SI

$
<

<

<
Ch

Ed

Cd

bo
C

-a

1 1

Ed

Ed

CO

Eh

bo
C

Eh

cu

CO

<

Ed
S3

&

<

1
ES

^*

c
(D
E

ES

fr.

Ed

aH 2
o^
ffl

1 1

<As

U CO

be

rl0
Ed

ca
a
Cd

8o
Eh

ca

o
Ch

Cd
CO

Cd

B
Cd

8
O
Eh

CO

Ed

n
<
S
Q
Ed

CO

V
CO

tt

-
0

13

T3

18

to

(N

o
CN

CO

0
V
>

fc
0

tf

O
U

Of

'ft

'&

CO

Si

ft

Hi

tN

fa

1a

-w

3S

Prod
For

eo

be

CO

"ft

Tw

&,

tie
Si

a
era

ss

ea

a.

u
H
a
a
+
a

c=

dition/
reatment

tt

g
2a
<:

Cd

ffi

gu

o
q

u
n

u
a
o

$
m
<

S3

fl H
o ^

ca

z
E
a

<

ca

s 3a s sa

CO

z
E

a
Cd
a

go

03

IS
Ed

ca
o
CO

CO

ca

Cd

a
o

a
<
o
o

g
E

a
a

<
<
fr-

3
a.&
id

a
z

<

>

J<

< g

6-7

Cd
CO
CO
Cd

a
a

CN

Cd

a
a

Cd

Cd

>>

9-

Cd

Cd

<:
s

Ed
CQ

CO

a
+

+
a

<
a
Q

(0

to

**

CN

CO

0>

tt

-w

18

Tfl

CN

13

73

V
>
SS

ti

CO

Ss
T?S
SH

eu

t)

CO

fa

c
E

cd

"a

13
cj
cd
h

5!

+
H
Q

8
as
a

en
03
63

Cd

B
3
Cd

Ed

P
CO

Q
Cd
J
J

o
OS

tn
Z

CN

SV
o
? td
S3

E03 fa

O E
B. <

RS
X

S
Cd

S
5

fa

8 2
2o

So
eB
? u

CN

O
m

te

8
IS

8.
a)

0.

<

Cd

CO

<
F-

ii

53

a
BB

g|

03

6-8

rf.

be

Ct,

lO

3
s
SI

8|

fa

i
S

,1

i*i
^

Cd

>-

>>

be

B
o

3B.

B. <

<

?K

au

be

CO

Cd

c- Cd
03

O E
03

a
3
O

S3
W

P.

fa
o

"CC

>

Cd
2
O

"

3
s

CQ

io

u
X

cd

Condition/
Heat Treatmen

CM

00

to

0)
a

-&

CM

CN

tt

-*a

-0

^3

T3

lO

t*

13

to

CN

c
o
E
a
'S

c
o
E

a
o
E

T3
CO

>

i-

U
tf

tt

H
Z
O
U

CO

&

bo
c

bo
e

fa

roduc
Form

CO

to

O
"8

bO
c

c
3

be
c

1 1

bo
c

&0
c

be
c
'be

be
c

CU
<
3
><BS

Condition/
Heat Treatme

e
<

<

<

I* BJ
IO 5
H o

fa
o

CN

<

fa

io

a
TO

<
s

o
Id

o
u

8u

ftn
<

a
Z

05

O
Q

&.
o
in

>^
< c

6-9

<

Of

CO

fa

9u

a
ES
B

M
H

I i

SB

en ~
03

03

ES

Pi

<

9u
z

8
>>
0

5
z

IO

1 1

6,

&.
o

BS
X

Q
cd
Q

CM

en

<

CO

en
CO

Ed

tt

13
13

tt

o
0

s.

Pu

<
H

a
o5
-a >
CH

s*
5B. 5ft.

Sz

? 2

s<

3z

fa >J

ss
Si

az
9 2

3z
o2

if

<

S
So

03

Is

SgS
a

"s

O ^

** Q

Si

Eg
S 5J
P. fc

#s

So

Q Z

gg

"" 2
u
_ 3
E a
a o

5fa ms
Cd
Z
Z

<

6-10

P0 o

<
Q2

on

O GO

si

S 3
a

63 #

I
S a

go

o
BS

Si
Ed ra
a
< Cd
SS

sg

o
tt

73

13

-
V
>
$4

p
p

tf

14

tt

H
Z
O

tt

co

CN

V
M

CO

CO

t*
C

ho
C

c
a

-a

tfi

CO

"3
cu

"5

m*

01

o
to

Conditi
Heat Trea

O -

BETA FINISHED
N TREATED &
1300F 2HR AC

IS

O or

IN-10 BETA BLOCKE


REDUCTION SOLUT
RAGED I650F IHR W

ti

be
C

g
a
a

CO

-a
v.

a
Cd
o

<3

u.
j

o
o
u
z

1
05

10
c~
to

<
U3 <

3g
< CN

05
o

Q b*

sfe

u
z
z

r^2
.a
E.

< 2

<
<
B

u
z
z

^H 56

a
a

<
<
fr-

<
<

Z
Z

Cl

<
S
o
&.

a
S3
S
p

9*

I
O
U3

6.
O

IS

IS

bo

la

CO

2",

eg

u <
B Bj

as
$1
of
z< a
B Z
Z

S.

8
"C
8.
c

CM

B 3
M

z z
z z

<<

u.
B

u.
a

B 5
=-

<
f-
H 8 <
a SB
J

LAB FOR-ANN BETA


BETA FORGED (1500
21 lit

Produc
Form

z
oa
Z B

5 o

fc

2
ig
< u
J a

<
a<

"a

>>
0

CN
CO

<

CO

6-11

<

z
z

BJ

<

X
B

D
a

tt

a
o
u
M

M
Hi

<
a
s

b
o
o
CO

X
w

o 5

<

ff

^r
<y

BS

as

5S

eH

8
05
S

O ^

<

<

s
>

9
9 c

3(5
CO w

6-12

*-

go

tt

-w

TJ

to

13

**

oo

15

03

73

>
h

C4

be
c

CO

P3

CD

o
CO

roduc
Form

&

'a

be

-a

bo

&

3
CO

T8
IC

'S
E

8.
5
3

be

&

"3
E

&

fci

H
O *

CO

E S3
E- o
a o

o2
u
S
CO
A

!<
< eg

S
5
O

"9 SS

fa ()8

o
3
m

>>

E-

P z
52

<
t-

Pz

BU HABFIN30STA BETA UPSET HI ALPHA


FINISHED 30% REDUCTION SOLUTIO
TREATED

ition/
eatment
T3

fi 8
BU B FIN-SOSTA BETA IJPSET BETA FINISH
S0% PRIMARY ALPHA !SOLUTION TREATED
AGED 1625F IHR AC1100F8HRAC

j^,..,

a
a
u
CO <

EJ 3
J

2
_
o
" CO

SB
< Q
E- Cd
Ed ca

5*
< o
E-

S
2 Xaa
z
CO
ft,

a Z

a ^
a
m

<

E- <
Ed Ed

az

52
5
a o
H CO
Ed Z

Si

<

<

CO o
O -

za
ft. x
g co

2z

<

<N

ES

EL.

S
EL.

o
U

<

8
IE

c
3

Ed O

ca Eg
a

8
2

CJ

ca a,

h
LO
(N
to

8
S
EL,

8
LO

i
LO

EL.

co
EL.

s
<

cj
EL.
EL.

CJ

<
ES

<
E3

ca

EL.

<

Of

EL.

S
t>

>
6
3

<
CO

6-13

<

<

ca

ca
a
CO

EL.

ca
a

CO

ft.

<

or

w
C4

u
a
ft. co

ft.

ft.

a
LO

00

CO

EL,

N ;3

<

S3
E- a

LO
tp-

to

& S5

LO
Cto

E3

gg
a|

EL.

3 E

CO

d cj
6. Z

o
o
00

CN

CO

K
-w
T5

^3

CN

"

CN

13

n
o
>

CO

co

bo

tie

IO

to

CD

fa

!
fa

3 S
fe
o o

10

CO
CG

CO

CO

Ed

*H fa

be

"6

rf

OH

ondition/
t Treatment

o
cd

<
u
fa
K

<
a

fa

fa

C3

<

fa
o

o
E-

<

Of

a
u
o
<
a

OS
X
IO

fa

^r

>
~ C
-1 o
< U
00 w

3
<

u
z
z

<

e
a
Ed

z
z
<

LO

i-S

os
s

EC

00

CO

0)

>>
0
<

00

<

<

os

CIS

<

fa
>
00

CO

CN

2
P

Ed
c
to
CN

<

to

*.

6-14

5?
a

fa
o

fa

to

Of

Of

Ed
Z
Z

<

03
B

fc

fa
8

3
C
CO
CN

>
<
CO

gs

"0
COQ

CO

|M

TO

CN

to

to

'

'

Min
Spec
Thk

HJ

'

OI

'

'

C4
CD

CO

&

to

COQ

J
H

O
f!
0)

0)
03

(3
0

TO

oi

Min
Spec
Thk

/^

LS
^5.
ST

o
**
w

s %
co a

tr

c
I

CM

CO

s
c

CO

.5 8*

S 02 P
^
-w

:
,

os

to

CN

CN

as

eft

*"

fX

TO
cS
o

CO

<r

CO

to

CO

e-

oi

eft

e>
o

CO

t-

io

04

CN

TO

s 8^*

IS

aTO

8
CO

oi

oi

io

ID

TO

CO

TO

te

en

TO

CO

OI

CD

CO

CO

"0"

(0

CO

CO

CO

CN

en

CN

tN
CO

o>

io

TO
t*
CO

TO

TO**"

CN

01

CO

OJ

to

l>

'

01

3
O

"

CO
to

c> s d 2
bpng^ d

oi

CO

jjj

CO

oi

S*g

bo

10

en

CO

CO

Eu

o
o

EBS

bo

be

V
CO

"6

1
s

bo

Vi En

OH

"n

+*

dition/
reatme

dH
9 *

<

ft.
i

(N
OS
<
free

&.
o

<:

C
CS
X
w

o
t>

a.
o

ft.

t-

C3

<

>>
0

U
Cd
CQ

<
Ed

<

CO

CO

6-15

ft.

o
o

O
H
U
b.

3
8

ft.

K
X
ft.
R

<

ft.
o

1<

PS

o
o

WS
=S <*

ft.

x 8
OJ

<
3 fti

u g
o

ft.
3
>
<
CO

cs

<

CO

ft. "
s

n
a

3
ft.

Cd
2
Z

ft]

<

<

ft.
S

<
Z
2

8
. Z
0

cop

10

CO

^"

0
CO

09

5
c

Min
Spec
Thk

03

'

*0
>
*s 0

a
0
-*

en a

5
a

c
s

.s 8-a

CO

*
*"*

^f

9
CO

CJ

to

ID
c&

!
1

CO

0)

t>"

(N

ft

ffi

to

eo

CO

eo

CO

0)
CO

GO

OS

CO

CO

CO

eo

CO

CO

CO

a s

CO

CO

CO

10

**

ao

oo

05
CO

tr

CO

10

eo

c-

Range of
Product
Thickness
(in.)

co e^

^,

0
10
eo
cGN

CN

eo

CO

C-

CO

eo

CO

CO

eo

10

CO

CN

GO

eo

0>

S
eo

8
CN

CO

CO

10
eo

s
**

CN

**

CO
N

as

CO

ON

CN

CN

CO

C9

0
iS >
9)
CO 0

P
Z
H
Z
O

S CO H

CO

0>

CM

*11

O
a

"

PS
O)
D

^* s
8

CN

CN

8
CO

04

CO

s0

CO

CO

-W

1M

a
C3

be

a
3
a

u
a

fa ELI

a
a

e
0

O
es

Ct3

fee
c

to
c

(9
ts

sm

be
C

01

PU

a
o g

<

S
co

*5 CO

10

d fa

0 ^

CO

ffl

p
Cd
O
Cd

<

CO

<

Ed %
O <

Ed

a
u

0 z

2Q
BETA
3 1950
SIZE

<a

CN
CO

CO
10

5s 8&

O O

<

g0

<

<

6-16

g t
<

(0

>
<

>>

CO
0

t1

3
Ed

>
c

<

CD

"0
to Q

c
a
J

03

,
*

.
'

,
'

'

'
1

CO
CO

**

t>
CO

^-

sie
c

w*
-+J

co

0)

h-1

A
V

eo

^"

O M

U3

.5 2
03

02

8 5
to a

so

00

*"*

(0

**

OS

coi

o u

so

w H

CO

so

g
v.*

CO

CN
CN

CO

t>

to

:
:

lO

to

CO

"*
ao

eo
U3

lO

CO

CO

CN

CO

IS

to

CO

CO

CO

c
<9
J2

Hi

._
ft **

U3

CO

CD
OJ
to

CO
Oi

CO

^*

CO

CO

tN

ao

"*

"

soi
5

ij

Cft

**

CO
to

CO

tD

i i

a.

CO

CN

e4

J2

ca

ca

&*
w

3s
o

a.

'&
rf

be

Vi fa

-a

&

ca

"eo

^
P3

tu

0
01

a.

h.

&
o
o

S8
u

2
2

<
<
S-

u
c

fa

fa

6.

Of

as cj
S <
us

u
B<
OJ

s <

fib

o
o

<

to

00 ^
BS

a
X

fa
o o

c
o *
T

BETA ANNEAL & S


0.BHRAC 1575F0.6H
8IIR AC

fc?

inge
rodu
ickn
(in.)

$
o

Conditi on/
Heat Trea tment

IS
ir

^-^

ffi

to a

3a

<

<

fa

z
z
Cd

fa
g
CO

<:
&

in
i>
to

t-

5
o
u
o
<
u

<

6-17

fa

C4

cr

OF

BS

fa
sto

fa
S
to

CN

>
<
to

<
BS
X

CO

>>
0

<
BS

3
c

CN

"8
S

CN

to

<

to

0
03

>4)
Q

"O

'

=L

'

CN

to
CO

(0

O
CO

t
CN

r-

c*
t>
o

CN

CN

CN

to

a
to

CM

C31

00

'

id

^ a
w 53

So*
9

o
o

.2
H

tf

to

B '
S =*

CO
CN

CO

,
'

10
CD

CO

c-

03 N
OS
0

P-4

ft

ss

09

a.

co
id

co

s ft
^

X
o

CN

> is *

m
a>

es

zz
eo

CN
r-i
C

cs*7 8^
00

CO
**

s
**

10

CO

0
CO

to
US

CO

to

C*3

02

o a

C
0)

*~

0.

CO

CD

pi

o
CO

CO

CN

CO

CO'

CN

cc

"S
o

Test
Temp
(F)

"* *"*

CO

2 &-~

PQ

"

CO

o>

Ei

J
fi

re

J)

J
r-

H
Ji

H
Jl

H
Jl

'

t^
05

f^
03

E^
S

-M

12 **a

3
"8 U

<H

,S

<

U 0a
ffl

>>
0

z
z

>
<

z
z

<

a:
CN

<

6-18

^H

J
U

>
<
to

<

CO

fi

>
9
P
-0
fa

08
as *}

13

^ ?

1
0

*u

g '
5 =

d.

50 N

cd
CO
B

ceo
^r

6
e

eo

x
2 1&.-2
13
fi g
s
.2
><i*

t^

en

4J

3.S
~

to

o
B

CD

Test
Temp
(P)

fa
O

f-

Jl

E-'
OS

tion/
atme

13

<
S

fa

IS H
0 ^

*-

0
h*

N*

>>
0

>
<
p

6-19

;K
:::::

*:>**':
*::

S3
6
CO

1 i

iilill
Z

co
to

-S3?

{*

01

01
CM

1|

11111

tH

CM

to
10

CO

CO
OJ

10

taq

CO

CO

CO

-4

llil , -o9
:

;.':;;:.**;

G* ^

|||s|S;;i|i

o
o

Iv ' '

6
o

o
:

ft

eo

t-

!*

GO

1
CO

Ed
W

<

CO

0)

<S

I
CD

c
D

ft

**

liijlti
S;!!

a
a
P
Z

TO

lO
CO
*

a.

Ifpitil
:

<:.

o
z

o
1=

<

><

>

Ti-6Al-4

CO

NDITI

O
CO

6-20

I
GO

e
D

I
e

CM

W<

*o
O
H

l
B
!

d
Z

llip

&

CO
01
pH

to

.>

10

ts

pH
pH

PH
PH

co
e*

to
co

to

oi

to

C4

SS

co
co
0

i?

ig*-*:

<9.

co

;S*pS;S;

in

*-4

IO

10
0

10
0

0
CO

CO

00

a
d

10

10

<y^

o
IM

ppllll
:

..::'::

io

..:.:;.:-'.''

0
PH

co

0
10

IO

OS

0
01

10

pH

co

10
pH

o
1-1

es

o
d

co
O

pH

c*
to

co

pH

pH

pH

5
a

CO
CO

CBOQ

E->
W
H
X

"g(X

s
D

CO

CQ

a,

OS

O
BS

Et.

Q
W
J

<

<
BS

OB
s^

fr

z
o
H
<
H

o
o

ia.

<

Ed

m
c

<

8u

ts

g
c
D

63

Ed

<

Eu
n
<

****

::x:x:::::::;$;:;:;:;:x:;:| S*:*:*

;S;J!;;$PS!:;;;

S
<:

H
X

<

><
O
T

03

13
IN

to

>
<
to

to

to

oi

*?
P

<
10
P

6-21

m
CM

IN

in
IO

CM

Sxdt&s::;
:

?S:::S^jS:

g
8

lili

d
o

<y

ifcllll

- o

5:5*:

00

oo
o

l-H

H
Z
O

to

IN

en

t^

co
o

i-t

CM
O

scd

OS

IO
CO

CO

lO

so

o
o

o
o

IO

IO

>*

GO
O

'

CM

CO
CO
<0

tCO

CO

l-t

""

rt

to
o

CO

f-4
4

CCM

to

8
C4

CM

g
o

1$;
:,

lip

CM

llftii

lllfll
1
HP

1H

z
s

to

c-i

CM

CO

IO

to

CM

IO
1-*

CO

*H

CM

CM

FV """f: X

lilllllll

o
T-l

CO

ii

i-i

w*

CO

CO

CO

o
o

5
5
CO
GO

es

CQ

55

o
35

=5

Ed

OS
a-

u
<

CO

CO

OB
if >
H
J

gg-j

EK

to
co

:<
H
Z

Ed
J

<

'V;<;/:"'.:

^raSp**^^

> -.
< =

6-22

<

to

<o

CO

l*

KS

ie

O
H
6

P|

to
00
C4
0*

Uli
o
O

in
1

**

0)

CO

?
3

8
K

<

CO

US

01

to
IO

CO
IN
01
CO

to
N

**

00

CO

IO
CO

i>
0)

CO

sd

IO
CO

co
cs

CO

co
00

IO

CO

C4
O

Oi
CO

CO

r-4

CO

IO
10

i#lti

:;

i-4

o
ii

t>
C*

lO

CO

CO

o
d

IO

C4

CO

IO

(N

o
d

CO
l-H

O
IN

o
o
!*

-v:.-;';

10

IN
O

M
o
d

o
d

g
a
CO
CO

CO

igiitii
ilillli

a,

3as

a.

H
w M

IZlIllll

Ed

OS

<

Ed
03
03
Ed

<
2

h3

o
H
^
H

8S

asfflamaMyaw

S3

iwS^iffiilftSI:

Z
C3

o
|
3 o

6-23

o
53

D
OS

Ed

1a

to

ilii*

CM

o
*K*S?

sif;
la
to

O
H

f
mm
iiii
lllllill

mm

3
e

c01

c-

CM
CO
CO
CM

co

illpSiS: :*:|:!:*:*
plSiS i*
cc

o
CM

CO

CM

CO
CM

CM

05

t-

io

CO

CM

CM

CCM
O
CM

0>
CM

CO
f-H

CO
CO

IO

rt

<-<

CM
CM

C~

"""*

10

SB

:&*-..

P5

CO

CO

CO

-r

5d

8o

CO

CO

CO

o
J,
o

IO
IO

CM

fH

#S

rl

o
d

o
o

8l|p^llli

IO

>

CM

X?

H
Z
O

CO

iiSpl*

IO

5?

eo

CO

eo
o

CO

g
3
o

63

CM

CM

o
d

o
d

2
O
co
3

0.

ft

|i;;5Ss!i

msmkm
og
55 Si

&s

Q
W

<

<s

OS

<

e
Ed

6-24

CO
CM

>

>
CO

CO

CO

H3
CM

Q
H
Q

P
O

Z
O

CO

W
M

6-25

e
o

CM

a
:

S:S:!
00

eo
CO

IS

"

z,

iill

1
ill
1

Hip
iiillli

IIlll

CO
1-

00
f<

CO

00

10
CO

;;

lO

CO

c-

CM

c~

-*

':

to

lO
O

CO

CO

CO
CM
O

lO
CM
O

to

o
o

sio

-*

o
o

e
eo
CO

C0

CO

CO

CO

t
o

eo
o

o
o

o
o

"'S

00

CO

o
eo

^^ilwgjjiwgs

CO

5
P
GO
CO

CO

IO

lO

CM

lO

CO

SSSSsS^sisg*

6
8

c-

rt

M
O

a
o

^1

2
O
ii
H
-<
H

gg
8

Q
Ed
-3

<

iS:;s:si;i;j!5gsss;:

SSSK

c
CG
LO

<
io

to

6-26

*
o

15
Ed

SS^Sigg:;::::::::

OS

EL.

<

I-*

CO

3
K

Q
Ed

-,

EEd
Ed
X
co

gg

-*

-*

10

Milli

CN

lO

lO

N
O

to

^4
-I

I
111

<0

CM

o
e

a*:!**
CO

III

'S*

*a

CO
S3

OS

IO

IO

IIH
&

llllll

*
d

fl
gggfew

eo

C4

CO

10

iq

to
CO

CO
CM

C3

CO
03

1-H

CO

CO

o
e

llHi

'"*

M.

llllpill

j^jr JTj

00

C4

ft

-t

-J

s
D

o
H

o
^4

o
vH

>o

d lllllili S~

z
o
CO

Si

Illllll

: PS";;

CO

cc

CO

Ed

W
GO

lllflll ipliiilf
Illllll
H^^^iS

S5

5>1
2^

Illllll g

<

g
3K
oIK

Ed
Q
3
Ed

Ed

CO
D
os

5Z
cu

BJ

flllllllll

<

p.

sa

Ed

Ed

g
Ed

Ed

S
Ed Ed
<

<es

Q Cd
Ed fe

Q S.

03 Z
Ed O

Ed X

Ed

>Ed ~
J
Ed
OS

CO

3Ed

&
<

OS

13

>
<to

6-27

sg

3OS
oEu

s
SEd

CS

Ed

>*
O

D
J
Ed

Ed
j

<

Ed

sa

Ed s
Q
J
Ed

Cd

Ed

O
Ed
Q
J
Ed

Illllll

Iz Illllll

J
Ed

HEAT1]

O
Ed

<

<os

3*
Ed
OS
X
co
Ed
05

Ed
c
o

5
<
CO

tIS'

a.

CO

M
Si

OS

IS

ca
xa

6-28

<N

S*;

s
o
so

a
'1

u
z I1

#|pi

co
to

9
CM

13;

IN

01
CM

pi

CM
CO
10

10
CM

10

01

c~

CM

CO
CM

CO
CM

*-*

CM
CM

CO
0

10
0

CO
0

CO
0

CO
0

10

CM
CO

s:;*?

<

LO

CO
CO

to

*?
w

&<*

,-<
o

wjjjftyS^vW'WIV ***"

CO

CO

es
oi

CM

01

OJ
CM
O

to

**

CO

to

pH

to

CO

o
d

to
0

^^ili

o
O
TH

IG

CO

I
CQ
CQ

CQ

CQ

l&SSx&SS:
lO

8-

o
d

lO

CO

CO

ipliiiii

lO

o
d

lO

C3
03

OS

fc,

; :
O

<

CM

<

05

<N

EL,

X
EL,

<

8
* X
u*
LO OS
,H

< Ex.
CO 8

es a
x
CM
EL.

8
to

to
CO

:::::::::::

::.-^^: >:v:': : : : : : : : : : : :

Of

CO

"Sa
to

0)
IS

CQ

2
a

cy

OS
X

o
o

Ct,

<-*
4

y. t.... y... .j.....................

z
o

a
d

EL.

EL,

Cd

CM

to

CO

lO

CM

CM

6-29

to

to

OS 0

x<

"-1 OS
X
8 00

03

EL.

to CM

10 *
t- oj

"* fc.

S En
OS
X
EL,

IO
CC-

5
5
to

lO
CM

o
w

U
2

to
IN
CD

***

Q
Q

lit

d
es

5K
o

cc

1-3

3
3
K
X

o
or

z
o

BS

I
Z

Io

>
O

<
to

SB

6-30

CO

: e

is

OH

<! S

egg
CO

fa

CO

IS

6
10

o
d

IS

I
: fa >?

CO
CO

CO

CO

MUMMMMMM

CO
I

c
D

I
z

I
a
10

6-31

4M

HI

&

lii

01

SWS

*<:;

i
O*

10

o
d

:*;*

U3

M
CO

CO

llitiil IHil 1111111

O
ob

Ed
IO

6-32

IO

if

dl

S 8

31

o
d

o
d

o
d

is*
0>HH

&8
o2
CO

HI

10

so
H

co

03

6-33

4-

mi

d
cd
W

Hi

00

SS
SWS

;:

ss

ig Si
CO

sei

ID

Ed

6-34

00

o
c

50)
2
<u
CO

t|

SH*S

SHOL DATA
MPEE TRE

02

HO
03 fa

J3
03

01
to

O ,5
O
TO

"3

<S

2
C

to
o

IO

id
IO

03 E-" ^

^O

is

s
t-

to

s?

N
IO

IO
CO

(N

^m

2
IN

SO

CO

03

CO

-i

J:

a
o

co

-i

-i

Fi

J)

E-

CO
-J

03
Ji

EJl

J
E*

e
o

C
o

CO

g,

CO
E-

J
E-

CO
E-

Ei
Jj

t-i

E-

S
a
C

J)

-i

8..S
c

S
o ,

'5

en

jr

Cd

CU

b.

b.

b.

Bw

u
o

<
s
OS
Ed
X
ECQ

i-

CQ

<
s

Cd

<

03
Q

OS
X
<N

<
b.
8

Eh
o
o

v-> es
O
EO
b.

2<
os
X
b.
o
o
o
Of

a
X
io

b<
b.

1
<
OS
X
w
Eh
o
io

<
os
X
CM
b.

CM

cy

Q
Ed

OS
O
Eh

1
ea

b.
o

IO
OS
X

<

<
s

CO

&.
CM

<
X
CU

<

aca
<
ca

O
OS

CU
Q
63

>

b3
U
Ed
OS
CO

<

IO

CM

EL.

o
b,

oa

a
J
J

OS
X

W
X
OS
X
CM
b. Q

8a.
a

<

1
a

>
<
to
p

6-35

OS
X
N
b.

a
j
w

Bca
b.
b<

<

63
X

os
X
b. S

si
w O

s
Ed

CU
Q
J
S3

CU
Q
Ed
=5
-C

8
363

<

S
t-

s
<

b3

b.

>

a
w

a
w

Ed
j

Jondition/
t Treatment

IS
RESS CORRO SIONC
R TITANIUM ALLOY

CO

e-S
o c $g

IHI

Q3

OO

-s

60 .p

sSis
o

>

fag

^8

18:

EH

o
c

oo
co

5a)

^_
0)
IO

DATA

mm

SHO]
MPE

I
m
a

SIONC
ALLOY

CD

CN

CO

o
m

S
00

CO
SO

TO

oi
10

<0

#5a

we

KOJ

-3

10

Tf

ia

111

:.E cx.S c
mm
o c
a

i
5

*
CD

j K

oo

>-3

o>

LTURE

1
J

:*: :*:$: :
:*:#*;

Sump
Tank
Water

b|

::

On

co 2

>o

CO

co
Jl

CO

CO

f-l

E-

6^

Jl

f-H

CM

00

rt

CO

CO
EH

J
E<

3m
E

<

<

<N

c
e-i

J
E

J
E-

CO

CO

E-

EJl

EJj

E-

J
H

3m
E

CO

-3
E-

->

3a
E

3
E

2CO

Sa
E

b.

3a
E

1H

I
Eb

f
u.

s
E

aa

CO

C
Ed

Bu
a.

<

a
CM

OS

Eb

u
<

E-

%%
K

<

o
o

g
33
<

OS

STRES!
FORTI

eo

CO
N

5 S
J ed

H
a
w

<
S

a
Eb

O -4-1

<
es

J
Ed
X
OS

BS

B!

a
CM

a
CM

Et,

Eb

CO

<y
0!

Of

a
o

CN

IO

<
05

a
CO
u.

**

cy

>

OS

a
O)
Cb
o
o

IO

8
00

o
cu
o
j
w
2:

Eb

<
a

05

a
Eb

~<

Eb
IO
CO

<

&H

u
c

>>

>~

en

J
Ed

>

s
>

O
CO

6-36

CO

>
6

i
oo

05

a
IO

Eb
IO
OJ

Eb

05

ci

CO
CM

'S
c
t-

,e
a>

2
Q)

s:
c

111
mm
o
*-

* a
Pfe
* >-s
'S

oE
X
K
X
o

rf

II
h
is

co H

lO

co S

c i

ffi H

Kg

a)

as

CM

co

CO

JJ

C4

CM

CO

t~

OO

is
^

2 CO

*J

3
o o
* fa

CO

X
as

<

SION
ALLO

>H

i
PH K

RESS
RTIT

o;z

HO

CO fa

<

Et.

in

<
>

>
o

Is

<

6-37

BETA

l&M&M

SSSSSSS;
WrSftttf

mm

* 0
OB -W
9 (8

Test
Time
(min)

HQ

SIS

fc

;s;li!il?

lO
CD
CN
00

o
C5
iH

rf5 mm

Prod
Thk
(in)

III!!
i

S3

JS

. !

>>>ivKvfc:>:::::

OS
fx

CO

o
o

mm

o
o

11!

S3

lll

i
$:-:-:::::::-:t::::::::

llllll
>

IC
CO

mm

mm

lO
CO
CN
00

IO
CD
CM

mmm

CD
3
CO
CN
00

' .: T-:

05
rH

IBS

ilpl ;V';0^
SU ls
r-t

: : : : : : : : :: : :

: : : : : : :A : : : :

:.:..:'::

05
TH

rt. '

IIII

CO

IAS m$m

df

"O S
ofa aS

t-

OS

TH

HI

i
i

'?

:
::>-(
i

oc

CD

+
00

OS

ssso;-

e lllll
Z
a
fa

03

SSSSSSS:

:tf:::x::

iiii

1
1

Hf

-.-.;'

wftvitv1:

i
i
i

ill

EH

2
:25
fa mm
to mm

si

All
s

:*:S::<5::

So
CO

:;^^;:

Z
fa
03

S
_< o
a-*

CN

CO

liiis

I
1
1

1
1

lliil HIP

:::::::::::::fc::::::::

1
1

:;:::::::v:::4:;::;::::

mmm

t
f

Illill
:I
85-i v/Z
w:$B$*$

:v::::::S3:::^:

1| 11
3&

30

00

III<
iicE:;
rH

All
!

i
i

CO
H

00

lO
CN

f->

w
CO

5Z

EH

fn

fa

iiiiSlil?

03

.So

*K35S3i

50 to

?"

i
i

8 es
o

1-1

E-5

03

E-!

c=5

E-;
05

E-J
05

00

03

03

03

03

CO

Cy

arxt

EH

E^

g
0
B
00

05
o

fa
P

CO
CO

fcft
B-S

fa

S
.

CO

e fa

111

j3CBg

Test
Temp
(F)

tf

lilll
-3.3

:..'-C>""

IP

>>:!:*::::::

Si 1

fa

00

CD

SJSSS

CN

g 3.S
O
0)
-

T-H

05

SSSSSS*

CP

*00

&

B
0

iwis

HIP
~<

&^:W:$:

(3

?
fats

CD

U3
CO
CM

^S$::i:

eo
w

lO
CO
CM
00

I;|;!;!;:;!;:::;;::::::::::

tf3
8

M
0<

mtts&s
ssssos*
sss:*;;

111:

ffiM

**\

;::;j:l:!:^;::;:;:x ::::%:i:WS

:;:l:l:l:!:!:!::;:j:lj-'

05

05

cy

EH

fa"5

fa-1
S* w

0
r l<

Tj< W

Tj" W

r-1

r-H

1-H

6-38

IB En

rH

03

<
H

fa
n

g
O

B,
BE

BETAC

J
CO

B >
1 Q

s
a s
&fi

ri

CN


to o

50

fcl

r4
-4J

,o

fl

.5
o

hJ

&

.0

tf

t>

c
J! W

05

fi

eo

m
T

CO

H
J

B >

to Q

t-i

r-(

CD

-W

fl

CO
0)

w
CO

<
CO

H
o
rt
+J

FH

73

-w

'

ou P
fa

o
a
C-

&

6-39

BETAC

We%.
&.
ssos

o
o
D

/-V

11

&

Hi

ca
CO

msmzm

1
II mm

ft;
H Illgfl
Z
p
H m&m

Z
O

50

es
ei

*<:

tf
|

0
C4

:!''> '' i:"*?

<y~
es

1-5

**.;;.-

^s

Q M' :

flft.

IPflll
H

H
Cd

S
CO

liMiili
A

'4.
O
KH
H
<
H
Z
H
1-4

:" z .

mmmm

lllii
Api
;:

- "}?,<':>"::':'"';;'

S
ipigiii

to

ZH
OH

6-40

BETA C

o
o

SSjfS!::

o
o

H
03

^
iilpi
llilgi

llltltl

W8M

III

7;

CO
C4

CO

:
CO

llllll

10

ti
M
^

o
IN

H
G^-s.
::::C?.-:-:-s^.-:-:-::-:-:-:::-:

CO
d

fc"'

*
CO
:: : :

::

: : : J2 ' ''^&--'''-'' -'-*-

O
C5

H
J
*
54
O
l-H
H
<
H

fc

&

....Z
A-

Zs

~5

CO

x->:LiJxC^:-x-:-::-:-::-:-:

I
6-41

BETAC

s
5>

>/;

rfan

g3
z
2go
u
a

CD

8a.

frei

SOB

00

i*
9?

so

E-

E-

ei*

2
p5
o
he

5cd
E

I
ft

6-42

This page intentionally left blank

6-43

^ BETA C I

Condition/Ht: STA
Form: 0.13 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: L-T
Frequency: 6 Hz
Environment: DRY AIR; RT
(1 of 2)

AK (MPaVin)
4

10

' I M'l'l

Yield Strength: 167.7 ksi


Ult. Strength: 183.5 ksi
Specimen Thk: 0.125 - 0.126 in.
Specimen Width: 6.002 - 6.026 in
Ref: 88575

40

100
1111

(2 of 2)

AK (MPaVin)
= I

' I 'I

10

10
o
o^10-4

\
c

-Z. 10

10

' I 'I'l'l

40

100

' I M'l'l

_i

Stress Ratio: 0.5

ZZ

_
_

__

10

2
io" ^
o
__
-3 p.
10 E
-

10

-^ 10 \

__

D
-5

-zz 10

10

-zz 10
10
4

10

40

100

I , I . 1.1.

1 , 1,1,1,

40

da/dN (10"6in/cycle)

AK (KsiVin)

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.164
0.301
0.624

5.37 (min)
6.
7.
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
41.22 (max)

RMS %
Error
22.15

10

AK (KsiVin)

AK (KsiVin)

1.07
1.62
2.26
4.56
7.40
12.3
21.6
37.1
63.5
110.
125.

Life Prediction Ratio Summary


-1

.5

RMS %
Error

.8

1.25

Life Prediction Ratio Summary


r-

0.

2.

Figure 6.2.3.1.1
6-44

.5

.8

1.25

BETA C
Condition/Ht: STA
Form: 0.12 - 0.13 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: LT
Frequency: 0.1 1 Hz
Environment: S.T.W.; RT

10

40

- I I I in'!
I
Stress Ratio: 0.1
10

100

I I <lllll

(2 of 2)

AK (MPaVin)

-I
10

10

b I ' I Tl'l

40

100

1 ' I 'I'll

Stress Ratio: 0.5

10

10

*"

10

10

10

_0J
"~

jv
o

o^10c
_

o
E

10

i/~

"

Jo

10
10

6^10"
W

210
10

Yield Strength: 167.7 ksi


Ult. Strength: 183.5 ksi
Specimen Thk: 0.116 - 0.127 in.
Specimen Width: 6.002 - 6.023 in
Ref: 88575

(1 of 2)

AK (MPaVin)

oy\

10

10
-7

10

10

10

10
10

"

, I,I,I,
4

I , LI,I,

10

40

10

da/dN (10"6in/cycle)

Life Prediction Ratio Summary


o + ex.

-1

0.

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.805
1.03
1.67
2.45
3.35
6.72
11.3
20.2
39.4
75.1
143.
271.
394.

6.58 (min)
7.
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
42.90 (max)

RMS %
Error
29.82

1111 n

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

LL1

1111ii

100

.5

RMS X
Error

Life Prediction Ratio Summary

r-

.8

1.25

0.

2.

Figure 6.2.3.1.2
6-45

.5

.8

1.25

1 BETA C I
Condition/Ht: STA
Form: 0.13 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: T-L
Frequency: 1 Hz
Environment: S.T.W.; RT
(1 of 1)

10

40

AK (MPaVin)
4

100

Stress Ratio: 0.1

10

10"

03

10

Z 10
\
o
~ -6
10

o
O-10-4
c

.-o
10 '\

10

10'2^

10

-=: 10

-6

10

I , I ,l,l,

10

40

Ill I

10

10

-r: 10

I , I,I,I,

10
4

100

RMS %
Error

da/dN (10"6in/cycle)

Life Prediction Ratio Summary


i

.5

.8

10

40

100

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

_fi I
10

10

- i .i,i,i,

Z 10
"a

T3

10

100

10

10

o
o 10

40

10

10

.2

10

I III I-

AK (MPaVin)
4

Yield Strength: 167.7 ksi


Ult. Strength: 183.5 ksi
Specimen Thk: 0.127 in.
Specimen Width: 6.009 in.
Ref: 88575

I III

RMS %
Error

Life Prediction Ratio Summary


i

1.25

da/dN (10"6in/cycle)

AK (KsiVin)

0.

2.

Figure 6.2.3.1.3
6-46

.5

.8

1.25

BETA III

N?
CC

"3

to

c
a

!
i

1.a

1-3

fef

CDQ

cc
c

eo

n >

iJ

2Q

e8
m

ao
o>

X"

-w

fl

0)

o
u

BJ

X
fx.

-w
CO
C>

(Y

fs
OS

10
IN

O
P4
W

b.
id
OJ

FH

T3
fl

4J

ISs

o o

a,

'S *
J* fc

CU

6-47

BETA III

is
rfj

^i'l
09

il^
*4
85

go

CO
CO

H
2*

|II
Si

&

<

P
g

E
fi

B
si

go

Se
CO Z
Z
o

o a

er
=> b

II
2 9

<*3

* H

fez

?5

*
feS

is

6-48

1
Is
H ES

This page intentionally left blank

6-49

EF

I BETA III I
Condition/Ht: STA
Form: 1 in. Plate
Specimen Type: CT
Orientation: TL
Stress Ratio: 0.1

Yield Strength:
Ult. Strength:
Specimen Thk: 1 in.
Specimen Width: 2.55 in.
Ref: 88144
(1 of 4)

AK (MPaVin)
4

- I

10

' I M'l'l

40

100

' I M'l'l

(2 of 4)

AK (MPaVin)
I

=]

Environment: Lab Air; -65"F; -q 1


Frequency: 0.1 Hz

10

' I M'l'l

40

100

' I M'l'l

Environment: Lab Air; 65T;


Frequency: 10. Hz

-=\ 10

10

10

10

10

10

10

_0J
_0J

o
\

-e-

o
6^10-4

-3 |

10

10"3E

-5

10

10

10

10

XI

10

10

10

10
10

10

10

10

10

i i 11 in
40
100

i i 111 n

10

10

I I I llll
4
10

da/dN (10"6in/cycle)

Life Prediction Ratio Summary


I-'

.5

.8

1.25

I I I 111

100

da/dN (I0"6in/cycle)

AK (KsiVin)

31.6
33.4
40.3
52.2
97.2
190.
333.

26.74 (min)
30.
35.
40.
50.
60.
68.42 (max)

RMS %
Error

J_J
40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

2.

RMS %
Error
31.39

Figure 6.3.3.1.1
6-50

Life Prediction Ratio Summary


.5

.8

1.25

H BETA III \
Condition/Ht: STA
Form: 1 in. Plate
Specimen Type: CT
Orientation: TL
Stress Ratio: 0.1

Yield Strength:
Ult. Strength:
Specimen Thk: 1 in.
Specimen Width: 2.55 in.
Ref: 88144
(3 of 4)

AK (MPaVin)
1

10

40

t I ' I 'I'l'l
-2

100

1 ' I 'I'l'l

Environment: Lab Air; 175F;


_ Frequency: 0.1 Hz

(4 of 4)

AK (MPaVin)

10

4
10
40
100
F=1i I i I'l'l
I ' I 'I'l'l
Environment: Lab Air; 175T; -rq 10
_ Frequency: 10. Hz

10

10

10

10
-3

.-3

10

10

io"2

_0)

_a>
o
o 10

o
o^10-4

_a
-H-

J3
-e-

10

"O

10

10

-3|
10 E

oP

"O

EF

-H-

^Jio \

10

10

10

10
10

10

10

10
10

LL

i 11HI

i i nn

10

40

10

LU
4

100

RMS %
Error

da/dN (10"6in/cycle)

100

r-

RMS %
Error

Life Prediction Ratio Summary


i

1.25

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary

.5 .8

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i i i nn

10

0.

2.

Figure 6.3.3.1.1 (Concluded)


6-51

.5

.8

1.25

2.

\ BETA III
Condition/Ht: STA E.B. WELDMENT (HAZ)
Form: Weldment
Specimen Type: CT
Orientation: TL
Stress Ratio: 0.1
Environment: LAB AIR;175F
(1 of 2)

AK (MPaVin)
4

10

=-J-l I in'!

Yield Strength:
Ult. Strength:
Specimen Thk: 1 in.
Specimen Width: 2.55 in.
Ref: 88144

40

100

I I I >lllll

Frequency: 0.1 Hz

(2 of 2)

AK (MPaVin)
1

10

I 'I'M

40

100

I 'I'l'l=1

10

Frequency: 10. Hz

-2

10

10

10

__

10

io"

6-10-4

"~"
_

-I

*^

10

_x"0

10

-3|
10 E

-3 |

10

-5

10

io"2
u

2 u

o 10
\

10

10

o
"

XI

10

&

10
-

10

10

10

10
II I I

10

T3

-el

10

10

I , I,LI,

10
4

10

40

10

RMS %
Error

da/dN (1()-6in/cycle)

0.

.5

.8

40

100

da/dN (I0"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


i

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , lilJ,

i i i nn

100

RMS %
Error

1.25

Figure 6.3.3.1.2
6-52

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

1 BETA II

EF

Condition/Ht: STA E.B. WELDMENT (WELD ZONE)


Form: Weldment
Yield Strength:
Specimen Type: CT
Ult. Strength:
Orientation: T-L
Specimen Thk: 1 in.
Stress Ratio: 0.1
Specimen Width: 2.55 in.
Ref: 88144
(1 of 1)

AK (MPaVin)
4

10

40

I 'I'l'lI

AK (MPaVin)
4

100

' I 'I'l'l

Environment: Lab Air; R.T.;


Frequency: 10. Hz

- I

10

' I 'I'l'l

40

100

' I 'I'l'l

-=\ 0

10

-2

10

10

10

10
10

10

_0>

10?
o

o
o^lO"4

o
6^10-4
\
c
_

,o4

10

z: 10

10

10

10

XI

"O

_,

10

10
10

10

10

10
'

i i i in
J_J

10

10

I i 11 h

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

.5

.8

1.25

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


0.

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error

D
T3

10

10

10

RMS %
Error

Life Prediction Ratio Summary


0.

2.

Figure 6.3.3.1.3
6-53

-\

.5

.8

1.25

^ BETA III I
Condition/Ht:
Environment: 0.6M KCI; 75F
Specimen Type: SENT
Orientation:
Yield Strength:
Ult. Strength:
(1

Kmax (MPaVin)
4

- I

10

' | 'I'l'l

40

Specimen Thk:
Specimen Width:
Ao:
Kjscc:
Ref: 82651

' I 'I'l'l

100

- Condition: Aged 900F 100hr

(2

Kmax (MPaVin)

3)

10

t I ' I 'I'l'l

40
1

3)

100

I 'I'l'l

Condition: Aged 1000F 100hr 10

10
10

10

10

10

Bawmff

10

10

-J10

10 2

I-

JC

Jl0

10

-dio

1 E

-A\o

\
1 E

10

10
10

-J10 >

D
XI

XJ

10

10

10

10
10

10

10

10

10

I'l'l'

10

10

I'i'i'

40

100

15.50 (min)
16.
20.
25.
30.
35.
40.
50.
59.50 (max)

I I.I ill

40

10

100

Kmax (KsiVin)

Kmax (KsiVin)
Kmax (KsiVin)

I ' Ml

Kmax (KsiVin)

da/dt (10"3in/hour)

23.00 (min)
25.
30.
35.
40.
50.
60.
70.
80.00 (max)

40679.
40511.
40187.
40656.
40950.
40700.
39904.
40560.
49207.

RMS %
Error
5.46

RMS %
Error
5.76

Figure 6.3.3.2.1
6-54

da/dt (10"3in/hour)
11248.
13585.
16206.
16046.
15283.
15101.
16587.
19711.
27111.

BETA III
Condition/Ht:
Environment: 0.6M KCI; 75T
Specimen Type: SENT
Orientation:
Yield Strength:
Ult. Strength:
Kmax (MPaVin)
1

4-

40
100
1i
I
i
MIM
b I ' I'l'l'l
-Condition: Aged 1250F 50hr

Specimen Thk:
Specimen Width:
Ao:
Kjscc:
Ref: 82651
(3 of 3)

Kmax (MPaVin)
4

10

10

I'l'l'l

40

100

1 I 'I'l'l

10
10

10

10

10

10

10
10

Jl i=r
c
-a

S-

^10

c
T3

10

10

10

10

-2 10

-1

10

10

-3

-3

10

10

10

10

10

n T>

10

"

5
o

SI

110 t_

'I

10

10

I I.I.I.

i i 11ii

10

. i 11 HI

I . I.I.I
40

1 00

Kmax (KsiVin)
Vin)

Kmax (Ksivin)
Vir
Kmax (KsiVin)

10

da/dt (10"3in/hour)

Kmax (KsiVin)

RMS %
Error

RMS %
Error

Figure 6.3.3.2.1 (Concluded)


6-55

da/dt (10"3in/hour)

BETA
Condition/Ht:
Environment: 0.6M KCI
Specimen Type: SENT
Orientation:
Yield Strength:
Ult. Strength:

Specimen Thk:
Specimen Width:
Ao:

Klscc:
Ref: 82651

(1

Kmax (MPaVin)
1

4-

10

' I 'I'l'l

40

100

' I 'I'l'l

- Condition: STA 900F 8hr

(2 of 3)

Kmax (MPaVin)

of 3>

10

b I ' I 'I'l'l

40

100

1 ' I 'I'l'l

Condition: STA 900F 40hr

-=i 1

10

10

10

10
101

10'

rwi
=10

110

10

I 10

io1 I

-M10"

_, -

10

-1

-1

10

10

10

10

10

n "O

10

10

_, 10

V-

^10"
o

I I I I ill
4

10

'

10

10

40

'

10

I I I III

100

10

I I HU

40

100

Kmax (Ksivin)

Kmax (KsiViin)
Kmax (KsiVin)

I I Mil

Kmax (KsiVin)

da/dt (10"3in/hour)

25.50 (min)
30.
35.
40.
50.
55.00 (max)

RMS %
Error
2.79

RMS %
Error

Figure 6.3.3.2.2
6-56

da/dt (10"3in/hour)
2289.
2995.
4400.
4516.
4466.
4381.

I nr-r \

Condition/Ht:
Environment: 0.6M KCI
Specimen Type: SENT
Orientation:
Yield Strength:
Ult. Strength:

- I

10

' I 'I'l'l

40

(3 of 3)

' I'l'l'l

_u
10

10

= I ' I 'I'l'l

40

100

' I 'I'l'l

_L

10

102

10

101

101

10

k-

10

L_

Jio

|io
\
c

\
c

_^

c>

*^_x

N_^

_,_, io~1

TJ

0 "^

10 \
a

T3

-2
10

-4-1

10

1
10"

10"3
-2

ID"2

10

" I , I,I,I,
1

10

m"4

I , l.l.h
40

r I , I,I,I,
1

1C)0

15.00 (min)
16.
20.
25.
30.
35.
40.
50.
56.00 (max)

10

I , l.l.l,
40

100

Kmax (Ksivin)

Kmax (Ksivin)
Kmax (KsiVin)

0-P
>
o
T3

-1

m-4

^-^

\
o
"<-2
10

10
10"3

,a'l

-M 10_1

\
~

II

Kmax (MPaVin)
4

100

-Condition: STA 900F 100hr

102

I III

Specimen Thk:
Specimen Width:
Ao:
Kiscc:
Ref: 82651

Kmax (MPaVm)
1

DL 1/

3
da/dt (10" in/hour)

Kmax (KsiVin)

36001.
35573.
35572.
36169.
35929.
35863.
36332.
35079.
42764.

RMS %
Error

RMS %
Error
4.61

Figure 6.3.3.2.2 (Concluded)


6-57

3
da/dt (10" in/hour)

BETA III

~]
::::::::: :::;:;:::;:::::;:

c
2o

S:i:;8

:888p::W:

:'*::'',
iSSSSOSw

ia

SiSSI^S*

MS

to

CO
CN
00

ssse*;*

i-< ..

rH

IM

mm

Si
iH
lO
CO
CN
00

-<
io

CO
<N

wmm

rH

ta

'

;:

a
<o
e>

'

CO
(N
00

SSSSCkSS;.

o
os

ii

iSills

* 9
09 -W

Test
Time
(min)

HO

O
%

'

T-

1-H

'V'x'--:

<

03
i-H

giiSpS*

i
i

1
1

.;:;.:-.0-:"
!!

1-1

i
i

' ''
!-*:

;:::::::::::::::+:;:;::::::

$:&::&*
o

^^

+
00
CM

?%:

11

;:J:-X;:;:;:;:':':':;:;:'::

Si.

i-l

ttttvttv**

1
CO

to:

CO

ft

IfIAS
SSSSOJSS

8
J4

SSSSSSSiS

* .s

ill

"5 pid ^

2.S fli

I
i

.*

CO
CO
CO
CD

H
d
o

.e
c W
~ Wft-KvftWft

3
9

Ilii

8a,

05

p4

<s

:ftv::::ic":ft::::::;

e C

CO

imWm
mmm

mm

3'&

H
2
H

03

C;

MS

ifc
2:
js

llili
Sj

oo S2

CO

lilll:

:SS?MJ$M

III

G s

Si

C& t-l

CN

H
0
as
S

2
&
0
a

a
0

g
0

09

0
o
0
09
09

CO

<0S

"2S **es

Sfe
CO
g
_, o

Ei

IO

"Sg
o a
3

j;i;^^^^:
xKIw::;:;:;:::;:;:
:":>>V:':y:
vS:S$:S::wB

::-:::::::::->:

ill

a
c
o

CUfc

BO

S Sfe

mwk
*

1
1

#:W:W&ftW:

:-:^S>^^W

"

1
1

^^JJw!

>^ O

: : : : : : : : :-:;:::;::

I
1

lllti

: ; : : :: : : :

lI
ail;;

+K

s
s
g

_g OS
a)
CQ

a
00
6-58

This page intentionally left blank

6-59

^ BETA Ti
Condition/Ht: BETA STABILIZED
Form: 0.16 in. Sheet
Specimen Type: CCP (max load specified)
Orientation:
Yield Strength: 136 ksi
Ult. Strength:
(1

Kmax (MPaVin)
1

10

40

Specimen Thk: 0.16 in.


Specimen Width: 8 in.
Ao:
Klscc: 68 ksi
Ref: 77456

of 1>

Kmax (MPaVin)
1

100

_ I 1 I llllll
1 1 1 >lllll
- Environment: 3.5 NaCI

-I
10

= I

' I M'l'lI

100

' I 'I'M

__

10

l-

c
-M10

X)

tz

o X>

10

10
_,

10

X)

10

10

10

10
-3

10

10

-w10

-3

10

-2

III 1

10

10

nG

40

10

10

10

10

10

10

10

1 , 1,1,1,

10
4

10

4lo

10
4

100

Kmax (Ksiviin)
Kmax (KsiVin)

10

0
40

100

Kmax (Ksivin)
Kmax (KsiVin)

da/dt (10~3in/hour)

RMS %
Error

RMS %
Error

Figure 6.4.3.2
6-60

da/dt (10"3in/hour)

CORONA 5
K

ufSL

81-

!**

CO

85

36.

a o so

00

ii*
9*?
Mg

el*
"l
P
D

a.

g
4

is

I
6-61

IMI834:

CM

i-H
CD
CO

6-62

This page intentionally left blank

6-63

\ IMI-834 I

Condition/Ht: 1864F 2HRS; OQ TO R.T.; AGE 1161F 2HRS


Form: Disk
Yield Strength: 100 ksi
Specimen Type: CT
Ult. Strength:
Orientation: C-R
Specimen Thk: 0.198 in.
Stress Ratio: 0.1
Specimen Width: 0.799 in.
Environment: LAB AIR;1099F
Ref:WL010
(1 of 1)

AK (MPaVin)
4

10

40

AK (MPaVin)
1

100

10

- I ' I 'I'l'l

40

100

1 ' I Tl'l=

10

10
10
10

_a)
o

io~2

o 10
c

,-f

Z. 10
T3

10

10
10
10
10
10

10

40

100

AK (KsiVin)
da/dN (10~6in/cycle)

AK (KsiVin)

0.

100

da/dN (10"6in/cycle)

AK (KsiVin)

11.6
14.6
19.3
33.7
43.5

Life Prediction Ratio Summary


i

40

1.54
2.15
414
6.34

7.62 (min)
8.
9.
10.
13.
16.
20.
25.
26.68 (max)

RMS %
Error
34.92

10

AK (KsiVin)

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


I

.5

2.
Figure 6.6.3.1.1
6-64

.8

1.25

This page intentionally left blank

6-65

\ IMI-834 I

"

Condition/Ht: 1864F 2HRS; OQ TO R.T.; AGE 1161F 2HRS


Yield Strength: 75-138 ksi
Form: Disk
Specimen Type: CT
Ult. Strength:
Orientation: C-R
Specimen Thk: 0.171 - 0.196 in.
Stress Ratio: 0.1
Specimen Width: 0.796 - 0.8 in.
Frequency: 1 Hz
Ref: WL010
(1 of 4)

AK (MPaVin)
1

10

40

-IM 'I'll

100

10

40
1

\=r-1i I i Ml'

1 ' I M'l'l

100

I M'l'l

Environment: Lab Air; 1099T; 10


_ Yield Strength: 75 Ksi

10

Environment: Lab Air; R.T.


_ Yield Strength: 138 Ksi

(2 of 4)

AK (MPaVin)

10
10
-3

10
<D

io~2

-3|
10
E

o
\

o"l0"
c
z 10

10

10
10
-7

10

10
10
4

10

40

100

AK (KsiVin)

RMS 55
Error
50.54

Life Prediction Ratio Summary


ED
I

0.

.5

T-

.8

100

0.640
0.808
1.31
1.91

4.60 (min)
5.
6.
7.
8.
9.
10.
13.
16.
20.
25.
26.25 (max)

0.0669
0.101
0.127
0.158
0.216
0.944
2.15
7.72
12.7

6.11 (min)
7.
8.
9.
10.
13.
16.
20.
23.04 (max)

40

da/dN (10'6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

10

AK (KsiVin)

i--

1.25

2.

RMS %
Error
32.51

Figure 6.6.3.1.2
6-66

2.60
3.33
4.10
6.39
8.38

10.3
11.4
11.5

Life Prediction Ratio Summary


AD
o
0.

.5

.8

1.25

2.

IMI-834
Condition/Ht: 1864F 2HRS; OQ TO R.T.; AGE 1161F 2HRS
Form: Disk
Yield Strength: 75 - 138 ksi
Specimen Type: CT
Ult. Strength:
Orientation: C-R
Specimen Thk: 0.171 - 0.196 in.
Stress Ratio: 0.1
Specimen Width: 0.796 - 0.8 in.
Frequency: 1 Hz
Ref: WL010
(3 of 4)

AK (MPaVin)
4

I
-2

10

40
1

' I 'I'l'l

(4 of 4)

AK (MPaVin)
4

100

- I

I 'I'l'l

10

I I 'I'l'l

40

100

' I 'I'l'l

-1

Environment: Lab Air; 1202T;


_ Yield Strength: 95 Ksi
-

Environment: Lab Air; 1099T; -=J 10


Yield Strength: 131 Ksi
^

10

10

10

10

10
a

o
10

io"2^

o
\

\
c

10

:
z: 10

i \f

_^"o
10

10

10

_nflP

10
o

10

10

10

10

10

10
4

10

40

~ I , I,I,I,
4

100

da/dN (10"6in/cycle)

AK (KsiVin)

.5

.8

100

2.34
2.36
3.15
4.80
5.64
6.54
8.52
12.8
15.5

8.97 (min)
9.
10.
13.
16.
20.
25.
30.
31.92 (max)

Life Prediction Ratio Summary


A
om
0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.500
0.839
1.97
3.44
4.99
8.54
10.5
13.0
19.5
34.2

6.56 (min)
7.
8.
9.
10.
13.
16.
20.
25.
29.62 (max)

I , hi,I,

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
38.87

1.25

RMS %
Error
49.26

Life Prediction Ratio Summary

Figure 6.6.3.1.2 (Concluded)


6-67

.5

r-

.8

1.25

iim
c

J
CO

ja o

ja

M
S
c

CDQ

1*

to

eo

fi
o
&

2 O

CS

.o>

.5
o

a0)

,o

(J
H

"8

tf

9)

co

H
J
50

Q >

coo
c
es
aM
M

PQ

to

lO

-(

il

e>3
in

CS
t-l

co

IQ

-w

-w

DA

<

0)

IX
00
b

C
CJ
-w

es

o
o
o

<
fa
K

<
a
X

o
*
**
>-<
TJ
C

&o

V
t>

-d b
o o

a
,

S- fe
PH

6-68

Ti-10-2-3

SftS
SSrJs
SSOK:
:& W*:

iS**:

o
JJ
&

111*!

s;****:*

H:K:g>SS4S;:;

Hill
lllil
iiiii
*<

o
o

CD

p$3:$

00

to

e
M

mil

^..::...-

iH
CO
CO

U3

'#

CO
CO
"

9
O
K

E
u
m

0.
to
2
D

ft\EB::::fcW::::::::Av::::ft:

SrH

zs
op

^3

s**M;5H;?^;^i

:**:*:*:
wssi

E
u
0.
2
2

O.CH

III

6-69

i Ti-10-2-3 I
Condition/Ht:

Yield Strength:
Ult. Strength:
Specimen Thk: 0.244 - 0.25 in.
Specimen Width: 1.991 - 2.006 in
Ref: NC005

Form:
Specimen Type: CT
Orientation: L-T
Frequency: 10 Hz
Environment: LAB AIR; RT
(1 of 3)

AK (MPaVin)
4

- I

10

i I M'l'l

40

100

10

Stress Ratio: 0.05

10

40

- I 'I 'I'l'l

' I 'l'l'l

(2 of 3)

AK (MPaVin)
100

I ' I Tl'l

Stress Ratio: 0.1

10

10

10

10
~"~

10

ID"3

10

_03

<D

2
10~ o
u
\

"""

_0>

o 10
-3 |

10

-Jio
>

-R .-6

10

m" ^
u
-o

-5

J2^r

10

in i

10

i , i.i.i,

10
10

40

II I I

10

-5

*""

10

10

10

I , l.l.l,

10
4

100

da/dN (10"6in/cycle)

AK (KsiVin)

9.03 (max)

Life Prediction Ratio Summary


en
r-

0.

.5

.8

100

0.664
0.689
1.16
4.68

8.93 (min)
9.
10.
13.
16.
16.40 (max)

9.16
23.3
24.0

9.

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.333
0.483
1.18
3.31

4.17 (min)
5.
6.
7.
8.

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
12.75

'

10

10

"~*

4 F
*E
v

Z 10
-a

ZL 10

-O

o
^10"+
c

1.25

RMS s
Error
3.46

Figure 6.8.3.1
6-70

25.4
34.3

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

r
>
-z
I T:
A r\
I ii 1 u z. v

Condition/Ht:
Form:
Specimen Type: CT
Orientation: LT
Frequency: 10 Hz
Environment: LAB AIR; RT

10

- I ' I 'I'l'l

(3 of 3>

40

100

I ' I Tl'l

- Stress Ratio: 0.33


~~"

AK (MPaVin)

"

ID"3 _

"

Kf'P
10 \
0

Bf

10

10 >
0
"O
-5

10

10

10-7

-^

-6

10

~ I , 1.1,1,
1

I , I

10

LLL

40

m"8

100

4.36 (min)
5.
6.
7.
8.
8.53 (max)

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.331
0.652
1 -75
4.85
15.3
40.0

Life Prediction Ratio Summary


a
0.

10

-6

10

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

1 . 1,1.1,

~ I , I,I,I,

AK (KsiVin)

4.46

-"

'

RMS SB
Error

vE

",-
10

ID"7

1ft-*

s-^
V

10"* &

-5

10

XI

-3

Z10"5

-6
10

_i

~ 10

0 10
\
c
^-^

100
.,.,.,

0)
0

S
B

10-3

Z10"5
-o
\

-1

io"2
S

40
|

a>

10
.|,,.,

10

10"2
-1

-"

<D

10

v-^

10"2

o^lO"
\
c

Yield Strength:
Ult. Strength:
Specimen Thk: 0.244 - 0.25 in.
Specimen Width: 1.991 - 2.006 in
Ref: NC005

AK (MPaVin)
1

.5

.8

1.25

2.

RMS 55
Error

Life Prediction Ratio Summary


0.

Figure 6.8.3.] L (Concluded)


6- 71

.5

.8

1.25

2.

Ti-4Al-3Mo-lV
0
0

o
00

2
.0

CO

lO
t-

<ts

3
o

* "a

JB

i-t

Test
Time
(min)

HQ

a>

CO
l

^^
fi

J^
M3

lO

o
1-H

^^

hfl
.*

0 o
ts fi

Prod
Thk
(in)

.M
0 o
fS

w
CO

Si

fi

fi

*~

as

fi

0
Q

*N

^s

>
fi

W>

o!

eo Z

h *9

fi

0 * .'S

0 h

s
a0
u

CQ

0,0
CO v

S fife

E-i

g
fi

+J
0
0

tf

o
fi
B
0

*<

&4

&< fe

OS
OS

s -s
e 0
S fac
H

O 0

OB

T3

fi

a>
a!

fi

0
0

a
IB

6-72

Ti-5-2.5 ELI

o'

;**;:
3S80H

ca

.
*iSsi|b

J^

ul

i-J

*tr

>\

o
o

**

a>

50

cc-

*H

>-

I1IS|
sssSsssiss::

III 111
111
an

-(

Z lllil

llltif

CO

CD

o
tf

V3

C~
H

lO

l-H

O*
i-l

SO

*:;*^

o
o

o
o

o
ftj 'F*4

to

fW

ti

Z
O

<

Z
H

isaiiii

1
SS

SSmj

[:
E
o
a
a.

to
2
D

ZH

8
III

6-73

Ti.5-2.5ELI
CM

*s
s'os

o"
SIOS

H
+

:'::.

SS*3K

CO
CO

fii

SOS

CO

mm

lull

is

c4
SO

111

mil
CD

Mil

Q
a
E
u
0.

6-74

TI-5-2.5ELI

CM

s>
o

':0

~<

o
o
5SK3K

S^S

CO
W

iplli
00

r-

to
00
00

OS

CO

3111

o
tt

liliii
m&lmm

8
llflfl

*1

&*

ja

~*

CD
,

'

o
d

IO

-H;i-.'"'':'-"

Ipllliil

IO

CO

3
03

ftt

o
l-(
H

4
H
Z

ilit|2*;:s

z
op

a
o
63

o
ZH
O c*

llltlflt

c
to

z
D

6-75

Ti-5-2.5 ELI

~+

PCI
O
H

o
o

SI*:

CO

0>
01

CM

CV

fa

3
5n

CO

13z

ii
CO
CO

fa

HH
PS tf
D
CO

IO

>

SSS**;

H3

us
o

CO

PUS

CO

CO

*<
<

o
P4

fa

CO fa

S
CD

fa
PQ

fa

o*^
fa N

_H

..

B::i,

13

o
o
Z
Q
fa

o
d

hH pH

fa
fa

Q
fa

to
Q

S
iligiii

c4i

liiliiiiii

CB

Pv

z
o

HH

3
H

Z
fa
PH

" z -

OS

;:

Ilpfailii
O

s
zS

E
w

t-t fa

CL.
CO

2
D

*S:-:;:$::

6-76

Ti-5-2.5 ELI

CM

iH

iS;
;*

H
:.

ill

CO

Ses

SwSS**;:

H
Z
l-H

H
Z

<
fa

HH

z
w

fa

CO
CO

WH
tf tf

Hp

co p
fa<

OK

iH

CD

1-3

S3QS

IN

a|

t-

/..

IplI

MiS
SSSjJifffiSS!

iiiill

ifii

oo
cco

b
*****

CO

co

CO

00

CO

a
o

us

o
tf

o^
3 N

g|
HH

wo

is
Ro

B PH
fa H

HS

H?
lO

CO
tf

Z
O
N*
H

z
fa

ao

&

z
fcg
OB
p*if|^Ssl;::

Q
H

w
CO

PfH

o5

llitiiiilt
ffi

6-77

Ti-5-2.5 ELI
:::::;:::;:::::;:;:;>;::o:o
::W::$;::%!::::::: i
:-::-::-:-:-::-::::::-:::

HM
*

CS

O
O

W&

/s

lii

iiiii

.*

io
CO

us
c~

io

IO

CO

_H

ijs3*f!ss;i

ilpti
S&S>K8

o
SS88SSB&

&4

8
Ilil

*
lJSli;:!;:;

JO
M

*,-.
ja N

50

-1

ei
::.fe

50

.:'...

v:',.:.:i-:

og
ji w

o
o

*o
o

o
o

to

5
lii

Pk
02

1
o

H
Z
siii

:*:%

IZliil $
OS

|S

a
E

5w
a.

2
3

III

6-78

U3

This page intentionally left blank

6-79

I Ti-5-2.5 ELI I
Condition/Ht:
Form: 3 in. Disk
Specimen Type: WOL
Orientation: R-C
Frequency: 0.1 Hz
Environment: LIQUID HYDR0GEN;-423F
(1 of 1)

AK (MPaVin)
1

- I

10

40

' I 'I'l'l

Yield Strength: 200 ksi


Ult. Strength: 211.1 ksi
Specimen Thk: 0.744 in.
Specimen Width: 2.002 in.
Ref: LG005
AK (MPaVin)
1

100

- I

' I 'I'l'l

10

40

' I 'I'l'l

100

' I 'I'l'l

10

Stress Ratio: 0.05

10

-2

10

10

10

10
10

_c;

O
frl0-+

10
_0J
o

10"

o
\

6^10-4
10

10"

a.

10

Z1010

'1
v

'

-z.

da

<u

< ~
m "\
o
x>

o
10

10
-5

10

10

10

10

10

10
'

10

' i
40

I'll

10

10
4

100

Life Prediction Ratio Summary


i

0.

100

3.15
7.47
11.8
16.4
28.3
69.1
72.1

13.30 (min)
16.
20.
25.
30.
35.
35.20 (max)

RMS %
Error
30.70

40

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (10-6in/cycle)

AK (KsiVin)

10

AK (KsiVin)

AK (KsiVin)

.5

RMS %
Error

r-

.8

Life Prediction Ratio Summary


0.

1.25

Figure 6.10.3.1.1
6-80

T-

-r-

.5

.8

1.25

2.

Ti-5-2.5 ELI
Condition/Ht:
Form: 3 in. Disk
Specimen Type: WOL
Orientation: R-C
Frequency: 10 Hz
Environment: LIQUID HYDR0GEN;-423T

4
10
I I I I 1 HI

Yield Strength: 200 ksi


Ult. Strength: 211.1 ksi
Specimen Thk: 0.745 - 0.748 in.
Specimen Width: 2.003 - 2.011 in
Ref: LG005

(1 of 2)

AK (MPaVin)

(2 of 2)

AK (MPaVin)

40
100
1I I I I MM

4
10
. | i|i|i|

40
100
i | >|i|i|

Stress Ratio: 0.5

10

10

_Q)
O

10

10

io"2

10

-Z. 10

o
9fc

10

-z.
10

o
x>

-s
10

10
10

10
4

10

40

" 1 , I.I.I.
4

100

da/dN (I0"6in/cycle)

16.
20.
25.
30.
35.
39.97 (max)

0.

.5 .8

1.25

0.990
1.13
1.51
4.01
9.48
21.3
27.1

8.44 (min)
9.
10.
13.
16.
20.
21.84 (max)

Life Prediction Ratio Summary


T

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.356
0.579
1.57
5.72
19.4
40.3
54.0
50.5

10.98 (min)
13.

RMS %
Error
>100.0

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i,i.i.i,

10

i-'

RMS %
Error

41.66

2.

Figure 6.10.3.1.2
6-81

Life Prediction Ratio Summary


i

.5

.8

1.25

i--

2.

i Ti-5-2.5 ELI hCondition/Ht:


Form: 3 in. Disk
Specimen Type: WOL
Orientation: R-C
Frequency: 0.1 Hz
Environment: LAB AIR; RT

Yield Strength: 113.6 ksi


Ult. Strength: 120 ksi
Specimen Thk: 0.746 - 0.749 in.
Specimen Width: 2.004 - 2.013 in
Ref: LG005
(1 of 2)

AK (MPcVin)
4

10

- I I '|'l'l

40

100

10

i I Tl'l

40

100
a

' | M'l'l

10

Stress Ratio: 0.5

-= 10

- Stress Ratio: 0.05

- I

I ' I Tl'l

(2 of 2)

AK (MPaVin)

10

10
**~

""

10

10
-3

10

10

^-*

2
io"

_Q3

6-10-4
c
_

-3

10

-5

zio

Z 10

/
/
0

10

2
10" o
o
\

-o

10

_R

10

-5

10"

-^

o
o

m^
u
x>

10

10

10

10

10
10

10

'1

"

1 ,1,1,1,

I , 1,1,1,
4

10

40

10

- 1 ,1,1,1,
4

100

49.57 (max)

RMS %
Error
13.44

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

1.99
1.98
2.07
2.35
4.21
7.97
16.8
21.5

7.78 (min)
8.
9.
10.
13.
16.
20.
21.59 (max)

3.52
6.43
11.4
19.3
30.1
46.2
70.8
164.

13.17 (min)

100

da/dN (10'6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

16.
20.
25.
30.
35.
40.

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

1 ,1,1,1,

10

2.

RMS %
Error
37.44

Figure 6.10.3.1.3
6-82

Life Prediction Ratio Summary


.5

.8

1.25

,-
2.

Ti-5-2.5 ELI
Condition/Ht:
Form: 3 in. Disk
Specimen Type: WOL
Orientation: RC
Frequency: 10 Hz
Environment: LAB AIR; RT

Yield Strength: 113.6 ksi


Ult. Strength: 120 ksi
Specimen Thk: 0.745 - 0.749 in.
Specimen Width: 2 - 2.005 in.
Ref: LG005
(1 of 2)

AK (MPaVin)
4
10
I I I I 'HI

40

100

69.25 (max)

RMS %
Error
9.74

0.

10

40

100

da/dN (10*6in/cycle)
1.09
1.14
1.87
2.76
6.17
10.5
17.8
30.9
51.8
86.6
96.3

7.91 (min)
8.
9.
10.
13.
16.
20.
25.
30.
35.
36.03 (max)

Life Prediction Ratio Summary


JB

100

1 ' I TIM

AK (KsiVin)

1.09
2.32
5.54
11.6
21.5
33.9
50.0
71.5
142.
283.
542.

16.
20.
25.
30.
35.
40.
50.
60.

40

AK (KsiVin)

da/dN (10"6in/cycle)

11.23 (min)
13.

10

b I ' I'l'l'l

AK (KsiVin)
AK (KsiVin)

(2 of 2)

AK (MPaVin)

40
100
1> I I | '|l|

10

1.25

RMS %
Error
23.13

Figure 6.10.3.1.4
6-83

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

\ Ti-5-2.5 ELI I
Condition/Ht:
Form: 3 in. Disk
Specimen Type: WOL
Orientation: CR
Frequency: 0.1 Hz
Environment: LIQUID HYDR0GEN;-423F
(1 of 1)

AK (MPcVin)
1

10

E~n"i 'I'll

40

Yield Strength: 200 ksi


Ult. Strength: 211.1 ksi
Specimen Thk: 0.749 in.
Specimen Width: 2.004 in.
Ref: LG005

AK (MPaVin)
1

100

i i'i'i'i

-1

40

100

1 ' I 'ITI

^~

10

10
10-3

10
~"

*~"

_K h10

J
t

o 10

<D

2
10" o
>>

6^10J

io" E
10

10"

"o

''

z: 10

2:

.BIIO

i T7

'\
U
-u

10

10

-7

10

10

-6

10

10
10

10

10

-o

10

- I ' I 'I'll

-= 10

- Stress Ratio: 0.05

zio

- i

,I,I,I,
4

i ,

10

-8

I,I,I,
40

10

100

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)

100

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


r-

0.

40

2.03
5.06
20.2
20.4
24.5
58.2
130.
135.

14.99 (min)
16.
20.
25.
30.
35.
40.
46.57 (max)

RMS %
Error
15.84

10

AK (KsiVin)

.5

i-'

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


i

0.

2.

Figure 6.10.3.1.5
6-84

.5 .8

1.25

I-'

2.

Ti-5-2.5 ELI
Condition/Ht:
Form: 3 in. Disk
Specimen Type: WOL
Orientation: CR
Frequency: 10 Hz
Environment: LIQUID HYDR0GEN;-423F

b I

10

' I Tl'l

40

Yield Strength: 200 ksi


Ult. Strength: 211.1 ksi
Specimen Thk: 0.744 - 0.747 in.
Specimen Width: 2.004 - 2.008 in
Ref: LG005

(1 of 2)

AK (MPaVin)

40

100

4
10
tl'l' I'l'l

100

da/dN (10*6in/cycle)

RMS %
Error
44.37

.8

10

40

100

1.25

da/dN (10"6in/cycle)
1.08
1.19
1.65
3.62
6.73
13.6
27.3

8.73 (min)
9.
10.
13.
16.
20.
24.45 (max)

Life Prediction Ratio Summary


.5

AK (KsiVin)

1.34
1.87
3.08
6.32
15.0
32.7
65.4
105.

10.10 (min)
13.
16.
20.
25.
30.
35.
38.83 (max)

40
100
' I 'HM

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

(2 of 2)

AK (MPaVin)

' I 'I'll

10

2.

RMS %
Error
41.95

Figure 6.10.3.1.6
6-85

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

~J 1 i 5-2.5

ELI I

Condition/Ht:
Form: 3 in. Disk
Specimen Type: WOL
Orientation: CR
Frequency: 0.1 Hz
Environment: LAB AIR; RT

Yield Strength: 113.6 ksi


Ult. Strength: 120 ksi
Specimen Thk: 0.745 - 0.748 in.
Specimen Width: 2.004 - 2.008 in.
Ref: LG005

AK (MPaVin)
4

1
_

10
l|l|>|

40
|

of 2)

-L

ID"2 _

io-2

io"

100

'|i |T|

-L

10

o
o

v_^

Z10"
D

-6
10
=

10

10

^__

\
o
~

>

-6
10

-6

10

i ,

m"6

I,I,I,
4

.8

10

40

~~

100

da/dN (I0"6in/cycle)

AK (KsiVin)
7.95 (min)
8.
9.
10.
13.
16.
20.
25.
25.45 (max)

2.30
5.11
12.3
9-06
1-28
0.0435
0.0101

I , LI,I,

AK (KsiVin)

da/dN (10'6in/cycle)

.5

>

-5

10"7

Life Prediction Ratio Summary


i

aa
~~^. 10

100

13.16 (min)
16.
20.
25.
30.
35.
36.74 (max)

0.

10

AK (KsiVin)
AK (KsiVin)

^-*

-z.

10

40

o
\
-3|
10 E

Z10"

-6

<o

io2

10

i
1

o
o 10
\
c

-5

I , I, !,l,

, Li,I,

-'

-z.
10

IQ"7

Q)

o
\

o
6-10-+
\
c

RMS %
Error
>100.0

40
|

la"3

<D

< "

10

| 1 |l|l|

10

ID"3

\
O
"

10

(D

Stress Ratio: 0.5

10

Stress Ratio: 0.05

100
l|l|>|

(2 of 2)

AK (MPaVin)

1.25

2.

RMS %
Error
45.63

Figure 6.10.3.1.7
6-86

1.57
1.59
2.15
2.79
5.25
8.68
15.3
28.5
30.0

Life Prediction Ratio Summary


0.

.5

.8

1.25

2.

H Ti-5-2.5 ELI
Condition/Ht:
Form: 3 in. Disk
Specimen Type: WOL
Orientation: C-R
Frequency: 10 Hz
Environment: LAB AIR; RT

Yield Strength: 113.6 ksi


Ult. Strength: 120 ksi
Specimen Thk: 0.744 - 0.753 in.
Specimen Width: 2.002 - 2.01 in.
Ref: LG005

(1

AK (MPaVin)
1

10

40

(2 of 2)

AK (MPaVin)

2)

100

10

El ' I'lTI

40

100

' I 'I'll

Stress Ratio: 0.5

-1

10

10
""""

10

10
JP
o

-r: 10

Z 10
a

"a

Jio
>

_B
10

~~

-5

10

10

10
,-B

10
4

10

40

9.
10.
13.
16.
20.
25.
30.
35.
40.
50.
59.86 (max)

RMS %
Error
50.67

142.
262.
325.
262.
159.
100.
107.
577.

Life Prediction Ratio Summary


0.

100

1.96
2.13
2.81
6.18
12.1
24.2
44.3
64.8
80.3
86.7

8.70 (min)
9.
10.
13.
16.
20.
25.
30.
35.
38.87 (max)

1.90
1.83
1.88
2.69
4.37
7.32
12.1
19.5
63.1

6.
7.
8.

40

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (10-6in/cycle)

3.89 (min)
4.
5.

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i , i.i.i,

- i ,i.i.i,

100

.5

.8

1.25

RMS %
Error
29.98

Figure 6.10.3.1.8
6-87

Life Prediction Ratio Summary


i

.5

.8

1.25

2.

\ Ti-5-2.5 ELI
Condition/Ht:
Form: 3 in. Disk
Specimen Type: WOL
Orientation: CR
Stress Ratio: 0.5
Environment: LAB AIR; RT

Yield Strength: 113.6 ksi


Ult. Strength: 120 ksi
Specimen Thk: 0.746 - 0.752 in.
Specimen Width: 2.006 - 2.012 in
Ref: LG005
(1 of 2)

AK (MPaVin)
4

_ I

10

. I llTl

40

100

10

-1

10

-3

40

100

Frequency: 1. Hz

10

10

10

10" o
o
\

~~

10~

-o _h10
_

jD

'1
z

Z 10

l_

'

1 T>

*\
u

"o

-5

10

"O

1
4

i 1 111 h
40
100

10

10

~ I , I . I. I.
4

RMS %
Error
81.47

.5

.8

40

100

da/dN (10~*in/cycle)
0.0555
0.0552
0.0672
0.120
0.213
0.744

24.90 (min)
25.
30.
35.
40.
46.12 (max)

0.212
0.197
0.855
10.4

Life Prediction Ratio Summary


0.

10

I , I,I,I,

10

AK (KsiVin)

da/dN (10"6in/cycle)

32.21 (min)
35.
40.
46.00 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

-5

10

III
1

.-8

,o4

-J10
>

_fi I
10
"~~

10

10

io'2

o 10
\
c

10
T>

10

10

10

10

_a>

-1

I I >I'l'i

Frequency: 0.02 Hz

(2 of 2)

AK (MPaVin)

1.25

RMS %
Error
12.91

Figure 6.10.3.1.9
6-88

Life Prediction Ratio Summary

.5 .8

1.25

Ti-5-2.5 ELI
Condition/Ht:
Form: 3 in. Disk
Specimen Type: WOL
Orientation: CS
Frequency: 10 Hz
Environment: LIQUID HYDROGEN;-423T

10

40

- i ' i 'i'i'i

-1

Yield Strength: 200 ksi


Ult. Strength: 211.1 ksi
Specimen Thk: 0.745 - 0.747 in.
Specimen Width: 2.006 - 2.012 in
Ref: LG005

(1 of 2)

AK (MPaVin)

(2 of 2)

AK (MPaVin)
1

100

10

40

100

40

100

' I * I 'I'l'l

I I I Mil

10

Stress Ratio: 0.05


10

10
10
o

o
O 10

10
TJ

10

-Jl0 >

, -O-

10

10
-7

10

10

I I Ulli

10

'I'll

10

40

100

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)
16.
20.
25.
30.
35.
38.28 (max)

RMS %
Error
32.43

1i

.5

.8

1.25

0.514
0.426
0.480
1.45

8.03 (min)
9.
10.
13.
16.
20.
24.09 (max)

Life Prediction Ratio Summary


0.

da/dN (10"6in/cycle)

AK (KsiVin)

3.18
3.56
5.40
9.69
20.5
50.8
99.7

15.02 (min)

10

AK (KsiVin)

2.

RMS %
Error
47.38

Figure 6.10.3.1.10
6-89

4.81
13.3
16.4

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

\ Ti-5-2.5 ELI fCondition/Ht:


Form: 3 in. Disk
Specimen Type: WOL
Orientation: CS
Frequency: 10 Hz
Environment: LAB AIR; RT

Yield Strength: 113.6 ksi


Ult. Strength: 120 ksi
Specimen Thk: 0.743 - 0.75 in.
Specimen Width: 2.004 - 2.01 in.
Ref: LG005
(1 of 2)

AK (MPaVin)
1

10

40

100

I ' I 'I'l'l
- i i M'i'ir
Stress Ratio: 0.05

(2 of 2)

AK (MPaVin)
4

10

b I ' I 'I'l'l

40

100

I ' I Tl"

10

10
10

10
2

IO~ P
o

o 10
c

|_
10

10

-5

10
"O

_. -

O
XI

10
10

10
10
-8

i I i I Mi
40
100

' l i lili
4
10

10

AK (KsiVin)

50.
60.
62.09 (max)

RMS %
Error
10.75

Life Prediction Ratio Summary


r-

0.

.5

r-

.8

100

0.582
0.577
0.454

7.98 (min)
8.
9.
10.
13.
16.
20.
25.
30.
35.
37.48 (max)

21.3
24.8
36.8
52.0
102.
207.
242.

28.32 (min)
30.
35.
40.

40

da/dN (10-6in/cycle)

AK (KsiVin)

da/dN (10*6in/cycle)

AK (KsiVin)

10

AK (KsiVin)

1.25

RMS %
Error
18.66

Figure 6.10.3.1.11
6-90

0.463
0.991
2.76
8.85
21.7
38.7
74.1
110.

Life Prediction Ratio Summary


i

.5

.8

1.25

Ti-5-2.5 ELI
Condition/Ht:
Form: 3 in. Disk
Specimen Type: WOL
Orientation: CS
Frequency: 0.1 Hz
Environment: LAB AIR; RT

Yield Strength: 113.6 ksi


Ult. Strength: 120 ksi
Specimen Thk: 0.749 in.
Specimen Width: 2.01 in.
Ref: LG005
(1 of 1)

AK (MPaVin)
4

10

40
1

AK (MPaVin)
1

100

I 'I'll

10

40

I 'I'l'l

100

' I TIM

10

-2

10

10
-3

10

o
frlo-4

10
10

_*T3
10
o

10
10
-7

10

10
10
4

10

40

'

da/dN (10_6in/cycle)

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.719
0.777
0.899
1.67
3.30
7.78

19.3
40.1
71.5
110.

Life Prediction Ratio Summary

RMS %
Error

Life Prediction Ratio Summary


i

0.

I I I III

40

0.718

7.95 (min)
8.
9.
10.
13.
16.
20.
25.
30.
35.
39.74 (max)

RMS %
Error
36.15

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I I Uli

100

.5

.8

0.

1.25

Figure 6.10.3.1.12
6-91

.5

.8

1.25

2.

\ Ti-5-2.5 ELI
Condition/Ht:
Form: 3 in. Disk
Specimen Type: WOL
Orientation: SC
Frequency: 10 Hz
Environment: LIQUID HYDR0GEN;-423F
(1 of 2)

AK (MPaVin)
1

b I

10

' I M'l'l

40

Yield Strength: 200 ksi


Ult. Strength: 211.1 ksi
Specimen Thk: 0.744 - 0.748 in.
Specimen Width: 2.004 - 2.005 in
Ref: LG005
(2 of 2)

AK (MPaVin)
4

100

= I

' I M'l'l

10

40

' I M'l'l

100

I M'l'l

10

Stress Ratio: 0.5


10

10
10

-no'2

u^10-4

10

-5

T>

10

10

-o

10
10
-7

10

10

10

40

100

RMS %
Error
54.15

.5

.8

100

0.0629
0.264
1.11
1.26
2.81
6.29
13.3

7.59 (min)
8.
9.
10.
13.
16.
19.69 (max)

1.38
1.49
2.31
5.00
12.3
25.0
41.1
56.1
65.8
65.7

Life Prediction Ratio Summary


0.

40

da/dN (10_6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

11.42 (min)
13.
16.
20.
25.
30.
35.
40.
50.
50.14 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I . I,I.I.

' i i mi

10

1.25

RMS %
Error
36.79

Figure 6.10.3.1.13
6-92

Life Prediction Ratio Summary


0.

.5

.8

1.25

Ti-5-2.5 ELI
Condition/Ht:
Form: 3 in. Disk
Specimen Type: WOL
Orientation: S-C
Frequency: 0.1 Hz
Environment: LAB AIR; RT

Yield Strength: 113.6 ksi


Ult. Strength: 120 ksi
Specimen Thk: 0.743 - 0.748 in.
Specimen Width: 2.005 - 2.01 in.
Ref: LG005
(1 of 2)

AK (MPaVin)
_

4
10
, i <|<n

-i

- Stress Ratio: 0.05

10

(2 of 2)

AK (MPaVin)
1

40
100
i | >|>|i|

4
10
prii | i |i|i|

40

100

40

100

-2

10

-3

10
JE
o
o 10
c

~~~

05

10
"O

T3

_. -

ion\
o

,m

10

T3
-5

10

10
10
10

~ 1 , 1,1,1,
4

1 , 1,1,1,

10

40

100

da/dN (10"6in/cycle)

AK (KsiVin)
13.
16.
20.
25.
30.
35.
40.
50.
52.94 (max)

RMS %
Error

27.79

.8

1.25

1.71
1.70
1.59
1.80
3.92
8.52
15.8
17.5

7.97 (min)
8.
9.
10.
13.
16.
20.
22.95 (max)

Life Prediction Ratio Summary


.5

da/dN (10"6in/cycle)

AK (KsiVin)

1.42
3.01
5.41
9.90
18.3
31.4
51.5
82.3
201.
258.

10.22 (min)

10

AK (KsiVin)

AK (KsiVin)

2.

RMS %
Error
60.56

Figure 6.10.3.1.14
6-93

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

\ Ti-5-2.5 ELI h~
Condition/Ht:
Form: 3 in. Disk
Specimen Type: WOL
Orientation: S-C
Frequency: 10 Hz
Environment: LAB AIR; RT

Yield Strength: 113.6 ksi


Ult. Strength: 120 ksi
Specimen Thk: 0.743 - 0.75 in.
Specimen Width: 2.003 - 2.012 in
Ref: LG005
(1 of 2)

AK (MPcVin)
4

10

40

(2 of 2)

AK (MPaVin)
4

100

- I

i I i I i|i|

10

40

I I Min

100

' I 'I'l'l

-I

Stress Ratio: 0.5

10

10

IQ"3

6^10-4
c

10

o
\
E

jS<*>

Z 10

-=

XI

CG

T3

10
10

10

10
-8

10
4

10

40

100

16.
20.
25.
30.
35.
40.
50.

60.
66.19 (max)

RMS %
Error
21.40

Life Prediction Ratio Summary


.5

.8

100

1.25

1.80
2.01
3.00
6.72
11.2
18.5
31.7
47.3

8.77 (min)
9.
10.
13.
16.
20.
25.
28.78 (max)

0.907
2.04
4.86
10.0
18.7
30.7
48.6
76.6
196.
534.
1019.

13.

40

da/dN (I0"6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

11.14 (min)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , 1,1,1,

- I , I, I,I,

2.

RMS %
Error
20.94

Figure 6.10.3.1.15
6-94

Life Prediction Ratio Summary


r- r~

.5

.8

1.25

Ti-5-2.5 ELI
Condition/Ht:
Form: 3 in. Disk
Specimen Type: WOL
Orientation: RS
Frequency: 10 Hz
Environment: LIQUID HYDR0GEN;-423F

10

40

Yield Strength: 200 ksi


Ult. Strength: 211.1 ksi
Specimen Thk: 0.745 - 0.749 in.
Specimen Width: 1.997 - 2.004 in
Ref: LG005

(1 of 2)

AK (MPcVin)

-I

10

~~

10"2^
o

(2 of 2)

AK (MPaVin)

100

_ I 1 I 'Pill
1 1 1 llllll
Stress Ratio: 0.05

10
i

i- I ' I 'IT
10

40
100
I i I mi

Stress Ratio: 0.5

-2

10

10
.9?
o
u 10

Z. 10

10

10

m
/
m

\
o

10

10
10
-8

10

~ i . i ,i.i,
4

1 ,1,1,1,

10

40

100

da/dN (10"6in/cycle)

AK (KsiVin)
13.
25.
30.

21.7
38.3

32.00 (max)

RMS %
Error
17.32

Life Prediction Ratio Summary


0.

.5

.8

100

0.306

7.79 (min)
8.
9.
10.
13.
16.
20.
25.
26.40 (max)

2.29
3.43
7.02

16.
20.

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.833
1.39

11.47 (min)

10

AK (KsiVin)

AK (KsiVin)

1.25

RMS %
Error
58.06

Figure 6.10.3.1.16
6-95

0.291
0.291

0.371
1.29
4.23
11.1
12.7
10.9

Life Prediction Ratio Summary


T-

r~

.5

.8

1.25

2.

\ Ti-5-2.5 ELI hCondition/Ht:


Form: 3 in. Disk
Specimen Type: WOL
Orientation: R-S
Frequency: 0.1 Hz
Environment: LAB AIR; RT

Yield Strength: 113.6 ksi


Ult. Strength: 120 ksi
Specimen Thk: 0.747 in.
Specimen Width: 2.001 - 2.002 in
Ref: LG005
(1 of 1)

AK (MPcVin)
4-

10

40

AK (MPaVin)
4

100

- I

10

' I 'I'l'l

40

100

' I 'l'l'l

10

Stress Ratio: 0.05

10

10

10

10

-3

10

10
Q)

10"2

_Q)

o 10

o^lO"
c
_

IU

10

10

Z 10

Z 10

\
o

icT\
o

"

T3

10

10

10

-o

-et-

10

10

10

10

10
10

I , I,I,I,

I , I , l.l,

40

10

10
4

100

AK (KsiVin)
da/dN (10-6in/cycle)

AK (KsiVin)

0.

100

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


i

40

0.447
0.442
0.616
1.30
3.78
11.5
25.4
41.4
52.1
53.0

9.84 (min)
10.
13.
16.
20.
25.
30.
35.
40.
40.84 (max)

RMS %
Error
65.02

10

AK (KsiVin)

.5

.8

RMS %
Error

Life Prediction Ratio Summary

i-'

1.25

2.

0.

Figure 6.10.3.1.17
6-96

.5

.8

1.25

2.

^ Ti-5-2.5 ELI r
Condition/Ht:
Form: 3 in. Disk
Specimen Type: WOL
Orientation: RS
Frequency: 10 Hz
Environment: LAB AIR; RT

Yield Strength: 113.6 ksi


Ult. Strength: 120 ksi
Specimen Thk: 0.744 - 0.748 in.
Specimen Width: 1.996 - 2.002 in
Ref: LG005
(1 of 2)

AK (MPaVin)
4

10

40
i

t I ' I 'IT

(2 of 2)

AK (MPaVin)
1

100

I i | i|i|

>- '

10

40

100

' I M'l'l

Stress Ratio: 0.05


-2

10

10

o
o 10

10

10

10

10
4

10

40

100

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error
31.83

100

0.691

8.18 (min)
9.
10.
13.
16.
20.
25.
28.08 (max)

0.0929
0.0830
0.175
0.639
3.48

17.6
47.5
73.4
73.7

0.757
0.933

2.25
5.44
13.6
26.6
31.9

71.9
212.
515.

Life Prediction Ratio Summary


0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.125

8.28 (min)
9.
10.
13.
16.
20.
25.
30.
35.
40.
50.
60.
64.25 (max)

10

AK (KsiVin)

.5

.8

1.25

i-'

2.

RMS %
Error
27.93

Figure 6.10.3.1.18
6-97

Life Prediction Ratio Summary


0.

.5

.8

1.25

2.

Ti-5-2.5 ELI I
Condition/Ht:
Form: 3 in. Disk
Specimen Type: WOL
Orientation: S-R
Frequency: 0.1 Hz
Environment: LIQUID HYDR0GEN;-423F
(1 of 2)

AK (MPcVin)
4

- I

10

' I M'l'l

40

Yield Strength: 200 ksi


Ult. Strength: 211.1 ksi
Specimen Thk: 0.746 in.
Specimen Width: 2.003 - 2.006 in,
Ref: LG005

100

Stress Ratio: 0.05

-Ml

' I M'l'l

10

10

40

i |i|i|

100
i|i|i|

Stress Ratio: 0.5

-2

10

(2 of 2)

AK (MPaVin)

-1

"

10

_a;
ho

6^10-4

o
o 10

_
-5

10

E
Z 10

10

_B

-o

10

TJ

-Jio
>

-o
10

fTUri

-3 10

10

" I , Mil
4

i ,I,I,I,

10

40

10

"I.I ,lrl,
4

100

da/dN (10"6in/cycle)

RMS %
Error
18.91

i-'

T-

.5

.8

40

100

1.25

da/dN (10"6in/cycle)
0.466
0.639

8.09 (min)
9.
10.
13.
16.
20.
22.27 (max)

Life Prediction Ratio Summary


0.

I , I,I,I,

10

AK (KsiVin)

0.942
1.00
1.89
5.56
15.4
24.1
24.5

12.00 (min)
13.
16.
20.
25.
30.
30.73 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

/'

10

10

-A-O

10

10

10

-3IE

tZ
-

-S2

10

XI

10

10

10

10

2.

RMS x
Error
>100.0

Figure 6.10.3.1.19
6-98

0.981
3.53
8.46
12.4
10.8

Life Prediction Ratio Summary


0.

.5

.8

1.25

Ti-5-2.5 ELI
Condition/Ht:
Form: 3 in. Disk
Specimen Type: WOL
Orientation: S-R
Frequency: 10 Hz
Environment: LIQUID HYDR0GEN;-423F

4
I

10

40

Yield Strength: 200 ksi


Ult. Strength: 211.1 ksi
Specimen Thk: 0.744 - 0.748 in.
Specimen Width: 2.004 - 2.011 in
Ref: LG005

(1 of 2)

AK (MPaVin)

(2 of 2)

AK (MPaVin)
4

100

= I

I 11 llll

10

40

I1

' I 'I'l'l

100

' I TIM

Stress Ratio: 0.5

10

10
10
10

\
-3 |

10

-AT>

10

T3

10
10
10
10

10

40

100

da/dN (10"6in/cycle)

RMS %
Error
90.92

Life Prediction Ratio Summary


.8

0.0505
0.261
1.02
1.32
3.13
5.42
11.0
9.71

7.49 (min)
8.
9.
10.
13.
16.
20.
20.73 (max)

10.0
20.2
38.4
70.6
79.4

.5

da/dN (10"6in/cycle)

AK (KsiVin)

0.376
0.863
1.95
4.42

10.74 (min)
13.
16.
20.
25.
30.
35.
40.
40.98 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I I I I ill
40
100

' I i I Hi

10
4

1.25

RMS %
Error
32.25

Figure 6.10.3.1.20
6-99

Life Prediction Ratio Summary


0.

.5

.8

1.25

1 Ti-5-2.5 ELI \Condition/Ht:


Form: 3 in. Disk
Specimen Type: WOL
Orientation: S-R
Frequency: 0.1 Hz
Environment: LAB AIR; RT

Yield Strength: 113.6 ksi


Ult. Strength: 120 ksi
Specimen Thk: 0.746 - 0.749 in.
Specimen Width: 2.004 - 2.009 in
Ref: LG005
(1

AK (MPaVin)
4-

- I

10

40

' I 'I'l'l

of 2)
4

100
_L

' I M'l'l

- I

Stress Ratio: 0.05


-

10

40

i I M'l'l

100

-1

' I 'I'l'l

10

Stress Ratio: 0.5

10

(2 of 2)

AK (MPaVin)

-2

10

10

10

"

o 10
c
Z. 10

-7

10

-8

10

_2

1
36

o
u 10
10

10"

10

1 . 1,1,1,

10

40

10
10

10

-8

10

35.29 (max)

RMS 95
Error
24.86

100

r~

.5

.8

10

40

100

AK (KsiVin)

1.25

da/dN (10-6in/cycle)

AK (KsiVin)

1.34
1.54
1.90
4.03
7.94
14.8
20.7

8.01 (min)
9.
10.
13.
16.
20.
24.82 (max)

Life Prediction Ratio Summary


0.

I , I, I,I,

- I , I, I,I,

1.45
3.42
8.45
18.9
32.3
45.7
46.5

35.

10

da/dN (10"6in/cycle)

13.07 (min)
16.
20.
25.
30.

m" ^
u

an 3

AK (KsiVin)
AK (KsiVin)

^-^

XI

_2

-I

z: 10

10

,lil,

- 1(T\
o

" I , I

a>
2
10"
u
\

or

10

10

_0J

RMS 95
Error
63.62

Figure 6.10.3.1.21
6-100

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

i-'

2.

^ Ti-5-2.5 ELI h
Condition/Ht:
Form: 3 in. Disk
Specimen Type: WOL
Orientation: S-R
Frequency: 10 Hz
Environment: LAB AIR; RT

Yield Strength: 113.6 ksi


Ult. Strength: 120 ksi
Specimen Thk: 0.745 - 0.747 in.
Specimen Width: 2.004 - 2.01 in.
Ref: LG005
(1 of 2)

AK (MPaVin)
1

10

i- i i Ti'ir
-I

40

= I
10

10

64.24 (max)

RMS %
Error
25.23

0.

.5

.8

10

10

40

100

1.25

da/dN (10"6in/cycle)

AK (KsiVin)

1.16
1.26
1.89
5.06
10.5
20.8
36.7
50.6

8.80 (min)
9.
10.
13.
16.
20.
25.
29.54 (max)

Life Prediction Ratio Summary


i

100

' I 'I'll

AK (KsiVin)

0.381
1.15
2.79
7.15
17.7
35.6
62.3
98.0
194.
315.
369.

16.
20.
25.
30.
35.
40.
50.
60.

40

' I M'l'l

100

da/dN (10"6in/cycle)

10.06 (min)
13.

10

Stress Ratio: 0.5

AK (KsiVin)
AK (KsiVin)

(2 of 2)

AK (MPaVin)

40
100
I I I INI

Stress Ratio: 0.05

2.

RMS %
Error
34.86

Figure 6.10.3.1.22
6-101

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

i-

2.

Ti-5Al-2.5Sn

;*KCK
e

::::

. ^*
O
O
to

O
CO

o
41

1
iiifjfliiit

o
.

*>
;lflliig iitpit
rnrnmm

mi

-<

*J"
GO

CO
CO

OJ
00

iiiiiii

R
p
..-*..

O
CO

il&ii;

O
3

CM

<5

::
N

&3 N

O
O

tfK
{^ w

50

10
0

CO
0
O

'-.'

U3
3

co

S*

: :: : : : : : ; : : :: : : : ; : : :

og

: : : : : : : : : : : : : : : : : : x :Q

?W

ill

I
H

III

H
fc

-.-H

op

111
0

[ 3

~t u

Zh

:::::

$
z
<j

RH
O ij*
ffi

6-102

Ti-5AJ-2.5Sn

tu
O

o
mat

-
0)

**
pH

wmm

1
.1

c-

c?

J3

SSKSSSSSS

o
o

Vt

GO
CO
CO

iiiif

M-l

$
*.

fc

IC

5
C*

tf
^
CNJ

ei

0*^

CO

,i '

CO

s*

PS
Sg

CO

SSrWivlfWA*:*:*:*:*

H
J

SgSi;

sift

14
O
HH
H
<
H
HH

tfB&S

H
Z

1
S"* >

ZH
OH

ill*
: : :: : : : :
::::::::

III
:**:?:

Q
H

HI

111

6-103

us

tCD

lTi-5Al-2.5Sn

;^:v:S:S^:;:::::;:::::;:

S&i&S:::::*:*::::
::::<:>:::'.::::::<

i-Iffii

O
H

1
Q

CO

gg

CO H

eo
TH

!D

tltpll

iiiii!

CO

id

o
d

MB*

CO

o
d

*3

ti

fa.

Z
O

: o

c*

8*3

02

:
*sa

O1^
:::::>:::::: ^^:-:^^-::::::

00
up

frt

H
J

Q
H

MH111B11

I
op

::'.::&.

III

<
H

CO

14
O

$S:

::-L .-OS ^

So:
::&"

:::-:-:::

^^;^SrW

s
og

si
H

sa

fill

1
Z

:-::&::

III
HI

6-104

CO

Ti-5Al-2.5Sn

o
<

::

00

cc

<o

S8
/-v

1
ills!

5
^

*.

CO

SSi*t*S*S*S

mmr-m-

111

<a

fllllll

ti

cvi

*<
&
o

**
c

<y^
o

CO

io
io

CO

Hill!
s
og
fij'

Eta
00

*^

fk

Z
I;^I1II
25
OB
s-f 5

^
M

ZH

3
a

OfH
Q^

til

6-105

Ti-5Al-2.5Sn

: O

.3

&i

IS
+

I
O
msam

i-5
T4
1H

CO

21

3i
111
:-0

Hi
mm

Pi ***
:-:-F*4v:^i'

HH

S
go
tf

QO

CO

EH

a
10

1
W

63

6-106

Ti-5Al-2.5Sn

o
o*
o

'

"

O
H

2
03

**

0>

:..'

cd

co

U3

as

o
::;:;:;:::::::SSIiii:

.5

iiii
0

.3

1
IM

:..

is*

CO

iiiiii
<3

iiilifcaS

CO

o
o

fc

z
o

*a
(M

tf

es
c4

r>
w

<y^
o

P^:-;-

CO

to

lllptil
: :

CO

og

ID

:EJj5>*:wW:::::::::::::::::>.

A*

&

o
H4

H
H

1110111

h-1

ms^m^^

<

NH

III
63

EC

111:

6-107

to
IO

CD

Ti-5Al-2.5Sn

I
o
*
s:
i&wfc

S8S:

^
T
H

<~v

tu

41
Q

till

IIII

iilpl

k*s

00
CO

tCO

M3

lllpll

la:

iiii
<

z
o
tf

<y^
o
P3

e4
CD

;v,r * -

a
N

Igpaiiii

CO
CO

to
to

tCD

cJ

Og

E
CO

iil^ll
HJ

&
S;**:!::

O
t-H
H
5
H

Z
H

. Z
Ipllll
liipni
pilil

iillpilll

6-108

Ti-5Al-2.5Sn

sses
#*

ssws

/-.
^
h

3 lllgl

H
Z

*rr

00

CD

-H

iiiaiii

>-t

00

TO

Wmm

llltli

CO

z
o
tf

w
M

w
oq
c4

O*^

co

Milli

i
a

CO
'..

CO

to

CO

M
&

;:P:s.'::-';

op
j

a
CO

H
Z

SrW

i^
lplil
-< ^ > '
CONDIT
HEATTRE/

14
O
N4
H
<
H
Z
H
ii

Q
H

3w
z

6-109

Ti-5I-2.5Sn
B

5>

1
rf!

rfl

is

j*

B
B

a
S

!U
p

SS
O

es

in
Sa

Hi

I
i*

o
z

9*5

3
fr

fr*

fr"

0. O
IE

K
00

s
a

Eh

ll

B
Z
Z

K
Z

z
z

<

<

6-110

z
z

<

Kl

z
z

<

i'Ti-5A]-2.5Sn

e
s

I
2>

is
t^S

rf

rfl
2>

10

IS

8a
CD

Is.
S*

H M
P. O

B3
5
B

oQ
0.

CQ u

5
g

Ed

z
<

<

6-111

<

SI

Ti-5Al-2.5Sii

l
5>
J* pa

fee

fi

rf

S3
P*H

is

'li

*B

5 So

25
CO

to

6.

IK

a
2*

gig
J

Bist

S5 c

1
s
Q

ro

51?
a

z
z

<

a
6-112

TU5Al-2.5Sn
as

I
5>

rf

1
rfl

is

J*

!!i
Bs

2
OS
IS

10

59
CO

17
laB n

5*

in
P. o

SJ

Sic
eg*

3 =

si

a
PL.

8g

2
2

<

z
2

<

6-113

a
2
2

<

a
2
2

<

2
2

<

B
Z
2

<

2
2

<

2
2

<

^ Ti-5AI-2.5Sn I
Condition/Ht: ANNEALED
Form: 0.08 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: LT
Stress Ratio: 0.1 - 0.67
Frequency: 30 - 55 Hz
(1 of 4)

AK (MPaVin)
4

10

40
I

i- I ' I 'IT

Yield Strength: 122.3 ksi


Ult. Strength: 133.9 ksi
Specimen Thk: 0.083 - 0.084 in.
Specimen Width: 2.754 - 2.764 in
Ref: 88911
(2 of 4)

AK (MPaVin)

100
i

I 111111

4
10
I i I in

40

100

' I 'I'll

Environment: Dry Argon; R.T.

Environment: Lab Air; R.T.

10

10

10
-3

10

10

o 10

G-10-4

10

Z. 10
-a

10

10

-7

10

10

10

10
4

10

40

100

AK (KsiVin)

RMS %
Error
2.77

-I-

.8

1.25

100

4.02
5.56
11.6
20.8
33.6
50.3
94.7
112.

18.13 (min)
20.
25.
30.
35.
40.
50.
53.17 (max)

8.92
11.6
21.3
34.5
51.2
71.2
124.
146.

Life Prediction Ratio Summary


0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

18.23 (min)
20.
25.
30.
35.
40.
50.
53.30 (max)

10

AK (KsiVin)

AK (KsiVin)

2.

RMS %
Error
4.05

Figure 6.11.3.1.1
6-114

Life Prediction Ratio Summary


an
i

0.

.5

1i

.8

1.25

2.

-\ Ti-5AI-2.5Sn h
Condition/Ht: ANNEALED
Form: 0.08 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: L-T

Yield Strength: 122.3 ksi


Ult. Strength: 133.9 ksi
Specimen Thk: 0.083 - 0.084 in.
Specimen Width: 2.754 - 2.764 in
Ref: 88911

Stress Ratio: 0.1


Frequency: 30 Hz
(3 of 4)

AK (MPaVin)

(4 of 4)

AK (MPaVin)
4

4
10
40
100
I I I i mi
I I I IM
Environment: Distilled Water; 10
R.T.

10

40

100

i I i |) j 11

t=~Ii I i I'M

3J

Environment: 3.5s NaCI; R.T.

10

10

10

10

10
10

10
2

io"

io'2

JE
o

o 10

frlCf
10

-3 IE

10

E
10

10

10
10

10

10

10
-7

10

10

10

10
i

10

i i 1111

10

I Mill!
4
10

10

40

100

da/dN (10*6in/cycle)

AK (KsiVin)

15.4
24.0
34.9
50.7
72.6
119.

20.00 (min)
25.
30.
35.
40.

53.14 (max)

152.

53.17 (max)

0.

.5

,
.8

,
1.25

29.9
51.4
69.2
86.0
105.
157.
179.

50.

Life Prediction Ratio Summary


-r-

da/dN (10'6in/cycle)

AK (KsiVin)

25.
30.
35.
40.
50.

21.49 (min)

i I I I Hi
40
100

AK (KsiVin)

AK (KsiVin)

RMS %
Error
3.20

,
2.

RMS %
Error
4.68

Life Prediction Ratio Summary


3
i

0.

Figure 6.11.3.1.1 (Concluded)


6-115

.5

.8

1.25

2.

H Ti-5AI-2.5Sn h
Condition/Ht: ANNEALED
Form: 0.08 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: LT
Stress Ratio: 0.1
Frequency: 50 Hz
(1

AK (MPaVin)
1

4
[=Ii

10

Yield Strength: 122.3 ksi


lilt. Strength: 133.9 ksi
Specimen Thk: 0.083 - 0.084 in.
Specimen Width: 2.754 - 2.756 in
Ref: 88911

40
100
i i 11 MM=q

I i |i|i|

Environment: Lab Air; R.T.

(2 of 4)

AK (MPaVin)

4)

= I

10

' I M'l'l

40

100

' I 'I'l'l

-"

Environment: Dry Argon; R.T.


10

10

-2

10

10"

10"

10

io"2

o
G^10"4
c
_

6^10"4

io

-5

Z 10

10
T3

0)

10

10

-=

x>

10

10"

-= 10

10

10

10"

10

10
.-8

10

i iiHi

10

40

10

h
100

.5

.8

1.25

100

2.12
4.77
10.0
17.3
28.6
38.7

16.59 (min)
20.
25.
30.
35.
38.01 (max)

Life Prediction Ratio Summary


a
0.

40

da/dN (I0_6in/cycle)

AK (KsiVin)

8.19
11.7
20.7
32.5
47.3
57.0

17.50 (min)
20.
25.
30.
35.
37.81 (max)

10

AK (KsiVin)

da/dN (10"6 in/cycle)

AK (KsiVin)

i , 1,1,1,

i I i I ill

AK (KsiVin)

RMS %
Error
1.82

-3|
10 E

io"*\
o

io"2"
o

RMS %
Error
4.62

Figure 6.11.3.1.2
6-116

Life Prediction Ratio Summary


H
I

0.

.5

.8

1.25

\ Ti-5AI-2.5Sn
Condition/Ht: ANNEALED
Form: 0.08 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: LT
Stress Ratio: 0.1
Frequency: 50 Hz
(3 of 4)

AK (MPaVin)
4
10
I I l I MM

-2

Yield Strength: 122.3 ksi


Ult. Strength: 133.9 ksi
Specimen Thk: 0.083 - 0.084 in.
Specimen Width: 2.754 - 2.756 in
Ref: 88911

40
100
Ti I i 11111

Environment: Distilled Water;


_
R.T.

1
zn

(4 of 4)

AK (MPaVin)

10

4
10
pn> i ' 11 MI

40
100
i I i I in

Environment: 3.5* NaCI; R.T.

-=i 1

10

10

10

10
-3

10

10
o

>^ .-*

o 10
10

10

-s

10

10
~o

-5

-=Jio >

\
o
"o

, -

, I
10

10

10

10
10

10

10

10
i l i
4

10

I I I I III
40
100

I I I I 111
4
10

10

da/dN (10"6in/cycle)

.5

.8

1.25

16.3
23.5
37.5
50.5
64.2
73.6

17.57 (min)
20.
25.
30.
35.
38.00 (max)

Life Prediction Ratio Summary


0.

da/dN (I0"6in/cycle)

AK (KsiVin)

7.49
11.8
20.4
31.1
42.4
52.7
56.3

.16.62 (min)
20.
25.
30.
35.
40.
42.00 (max)

RMS %
Error
7.49

LiL

I I I llll
40
100

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

\A

2.

RMS %
Error
4.55

Life Prediction Ratio Summary


cm
i

0.

Figure 6.11.3.1.2 (Concluded)


6-117

.5

.8

1.25

2.

-I Ti-5AI-2.5Sn r
Condition/Ht: ANNEALED
Form: 0.08 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: LT
Stress Ratio: 0.67
Frequency: 55 58.3 Hz
(1 of 4)

AK (MPaVin)
4

E I

10

' I M'l'l

40

Yield Strength: 122.3 ksi


Ult. Strength: 133.9 ksi
Specimen Thk: 0.083 - 0.085 in.
Specimen Width: 2.752 - 2.756 in
Ref: 88911

4
10
P=Ii I i Ml'
FT

100
a

' I M'l'l

10

Environment: Lab Air; R.T.

(2 of 4)

AK (MPaVin)
40

100

I I I I'l'l

Environment: Dry Argon; R.T.

10

10

10

10

-3

10

10

_Q3

io"2

u 10

fri o"
c

zio

-3 |

10

10

Jio
>

x>

x>
10

Z 10
-o
\
o
"
-6
10

10

<X
10

10

10

10
10

10

10

, I , l.l,
4

i 1 i 1111

10

40

'

10

100

da/dN (10"6in/cycle)

RMS %
Error
14.65

0.

.5

.8

0.0559

0.0796
0.138

9.
10.
11.87 (max)

1.46
2.17
5.55

0.0301
0.0443

6.
7.
8.

0.937

100

0.0150

4.31 (min)
5.

0.0610
0.151
0.310
0.563

Life Prediction Ratio Summary


,

i iiHI

40

da/dN (10"6In/cycle)

AK (KsiVin)

0.0604

3.99 (min)
4.
5.
6.
7.
8.
9.
10.
12.86 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'

i i 11 ii

no
1

1.25

2.

RMS %
Error
18.52

Figure 6.11.3.1.3
6-118

0.269
0.999

Life Prediction Ratio Summary


4DA +
-I-

0.

.5

.8

1.25

2.

^ Ti-5AI-2.5Sn r
Condition/Ht: ANNEALED
Form: 0.08 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: L-T
Stress Ratio: 0.67
Frequency: 55 58.3 Hz
(3 of 4)

AK (MPaVin)
4

10

40

Yield Strength: 122.3 ksi


Ult. Strength: 133.9 ksi
Specimen Thk: 0.083 - 0.085 in.
Specimen Width: 2.752 - 2.756 in
Ref: 88911

100

10

40
1

r=lr-r-r

' I M'l'l

I ' I M'l'l

Environment: Distilled Water;


R.T.

(4 of 4)

AK (MPaVin)

10

100

I M'l'l

- Environment: 3.5s NaCI; R.T.

10

10
10
10

io~2

10

10

10
10
-o

_B
10
10
10
10
10
4

10

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error
8.05

0.249
0.530
1.01
1.68
2.49
3.38
6.36

i-'

.5

.8

100

1.25

0.124
0.149
0.295
0.723
2.29
5.45
7.25
7.38
11.3

3.77 (min)
4.
5.
6.
7.
8.
9.
10.
12.93 (max)

Life Prediction Ratio Summary


-as
0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.0777
0.0804
0.113

3.44 (min)
3.5
4.
5.
6.
7.
8.
9.
10.
12.87 (max)

10

AK (KsiVin)

AK (KsiVin)

2.

RMS %
Error
12.68

Life Prediction Ratio Summary


i

0.

Figure 6.11.3.1.3 (Concluded)


6-119

.5

.8

1.25

2.

^ Ti-5AI-2.5Sn r
Condition/Ht: ANNEALED
Form: 0.08 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: T-L
Stress Ratio: 0.1
Frequency: 30 Hz
f

AK (MPaVin)
10

- I

I I llll'l

40

Yield Strength: 125.4 ksi


Ult. Strength: 133.9 - 135.2 ksi
Specimen Thk: 0.083 - 0.085 in.
Specimen Width: 2.753 - 2.757 in
Ref: 88911

4)

-1

- I

10

Environment: Lab Air; R.T.

-2

10

10

-3

10

io"

10

<o

10"
o
2

_o
l

o
o^10-4
\
c
_

10~

z: 10

ZM0

T3

"o

10

("
10 '\
u

_,
10

10

10

1
^-^
z

/
/

_c

.-6

-7

10

10

-6

-6

10

M0

10

10

10

"O

-1

"""

o 10
\
c

' I M'l'l

Environment: Dry Argon; R.T.

10

ID"3

40
100
' I M'l'l
-1

10

100

' I M'l'l

(2 of 4)

AK (MPaVin)

" 1 ,). f, 1,

! r 1,1,1,
40

10

10

- i , M.I,

RMS %
Error
4.41

.5

.8

da/dN (10"6in/cycle)

AK (KsiVin)

3.92
5.38
12.4
22.1
35.3
53.7
114.
143.

18.62 (min)
20.
25.
30.
35.
40.
50.
53.29 (max)

10.7
11.2
23.9
35.9
54.0
79.6
140.
167.

Life Prediction Ratio Summary


0.

100

AK (KsiVin)

da/dN (10"6in/cycle)

19.82 (min)
20.
25.
30.
35.
40.
50.
53.22 (max)

40

10

100

AK (KsiVin)
AK (KsiVin)

i , I,I,I,

RMS %

Error
9.16

1.25

Figure 6.11.3.1.4
6-120

Life Prediction Ratio Summary


o
r-

0.

.5

1-

.8

1.25

2.

^ Ti-5AI-2.5Sn
Condition/Ht: ANNEALED
Form: 0.08 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: TL
Stress Ratio: 0.1
Frequency: 30 Hz
(3 of 4)

AK (MPaVin)
1

- I

10

Yield Strength: 125.4 ksi


Ult. Strength: 133.9 - 135.2 ksi
Specimen Thk: 0.083 - 0.085 in.
Specimen Width: 2.753 - 2.757 in
Ref: 88911

40
100
TI I I I Mil

' I 'I'l'l

Environment: Distilled Water;


_
R.T.

(4 of 4)

AK (MPaVin)
10

40

100

Environment: 3.5SB NaCI; R.T.

-r=j 10
-2

10

10

-= 10

10

10

10

.2?

10

Z 10

10
T3

10

-o

J?

^10"4
\
c
_

o 10

10"

10"

-=

"O

'

_K -

o
\

("
'\
u

_K

10

10

-= 10

10

10

10

-= 10

10

10

'

I 11II

10

I I 11 ll

40

10

" 1 ,1,1,1,
4

100

da/dN (10"6?n/cycle)

177.
201.

53.13 (max)

148.

Life Prediction Ratio Summary


0.

34.7
50.0
68.0
85.7
109.

25.
30.
35.
40.
50.

130.

53.08 (max)

RMS %
Error
5.01

100

da/dN (10"6in/cycle)

AK (KsiVin)
21.52 (min)

9.47
12.5
23.6
38.6
57.3
79.0

18.18 (min)
20.
25.
30.
35.
40.

50.

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i,i.i.i,

10

.5

.8

1.25

2.

RMS %
Error
16.36

Life Prediction Ratio Summary


o
,

0.

Figure 6.11.3.1.4 (Concluded)


6-121

.5

.8

1.25

2.

^ Ti-5AI-2.5Sn h
Condition/Ht: ANNEALED
Form: 0.08 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: TL
Stress Ratio: 0.1
Frequency: 50 - 53.3 Hz
(1 of 4)

AK (MPaVm)
1

- I

10

' I 'I'l'l

40

1
10

_Q>
O

A
=

&
&

io" "
4

O^IO"

10

10~

I , I,LI,

10

40

10
10

'

10

RMS X
Error
4.83

AK (KsiVin)

r-

.5 .8

I llll

40

100

1.25

da/dN (10"6in/cycle)
3.20
5.37
11.7
21.2
34.7
44.6

17.46 (min)
20.
25.
30.
35.
37.87 (max)

Life Prediction Ratio Summary


o
0.

10

AK (KsiVin)

7.03
11.8
20.2
31.1
46.5
59.5

I I 11 ll

100

da/dN (10*6in/cycle)

16.63 (min)
20.
25.
30.
35.
38.10 (max)

4 "
'\
u
x>

10

AK (KsiVin)
AK (KsiVin)

'

10

10

" I , l,U,

.-8

10

4
z.

10
10

10"
o
\

XI

10

10

-7

10

10

-5

10

100

' I M'l'l

10

Z 10

40

-2

^10"4
\
c
_

10

' I M'l'l

Environment: Dry Argon; R.T.

10

10

b I

_L

' I M'l'l

(2 of 4)

AK (MPaVin)

100

Environment: Lab Air; R.T.

10

Yield Strength: 125.4 ksi


Ult. Strength: 133.9 - 135.2 ksi
Specimen Thk: 0.083 - 0.085 in.
Specimen Width: 2.755 - 2.756 in
Ref: 88911

RMS %
Error
3.70

Figure 6.11.3.1.5
6-122

Life Prediction Ratio Summary


o
~r~

0.

.8

1.25

H Ti-5AI-2.5Sn h
Condition/Ht: ANNEALED
Form: 0.08 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: TL
Stress Ratio: 0.1
Frequency: 50 - 53.3 Hz
(3

AK (MPaVin)
4

10

40

I1

- "1 ' I M'l'l

Yield Strength: 125.4 ksi


Ult. Strength: 133.9 - 135.2 ksi
Specimen Thk: 0.083 - 0.085 in.
Specimen Width: 2.755 - 2.756 in
Ref: 88911

100

' 1I M'l'l

Environment: Distilled Water;


_ R.T.

10

40

I 11\'\'\

10

10

"""

10

10

-3

IQ"3

10

_a>

.2
t
o
6-10-4
\
c
_

10"2

O
4

6-10-

,0*1

/
10 \
o

-3

10"3E

_^xi

2 10"'
"o

10

10

T3

_.
10

10

~~~

-= 10

10

10

II 1 1

10

100

' I 'l'l'l

Environment: 3.5SB NaCI; R.T.


10

10

(4 of 4)

AK (MPaVin)

4)

10

10

i ,

10
4

10

I,I,I,
40

10

100

RMS %
Error
5.76

.5

.8

1.25

14.2
24.4
39.3
53.4
69.6
79.0

16.28 (min)
20.
25.
30.
35.
37.84 (max)

Life Prediction Ratio Summary


on
i

da/dN (10-6in/cycle)

AK (KsiVin)

7.01
12.0
21.3
33.4
49.2
59.9

r~

100

AK (KsiVin)

da/dN (10"6in/cycle)

16.57 (min)
20.
25.
30.
35.
37.79 (max)

40

10

AK (KsiVin)
AK (KsiVin)

I , Ml

" I , I,I,I,

2.

RMS %
Error
5.01

Life Prediction Ratio Summary


i

0.

Figure 6.11.3.1.5 (Concluded)


6-123

.5

.8

1.25

2.

H Ti-5AI-2.5Sn r
Condition/Ht: ANNEALED
Form: 0.08 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: T-L
Stress Ratio: 0.67
Frequency: 54.2 - 58.3 Hz
(1 of 4)

AK (MPaVin)
4

1
1

10

Yield Strength: 125.4 ksi


Ult. Strength: 133.9 - 135.2 ksi
Specimen Thk: 0.083 - 0.085 in.
Specimen Width: 2.753 - 2.757 in
Ref: 88911

40
100
i I i i 11' I

I 'IT

(2 of 4)

AK (MPaVin)
- I

10

' I M'l'l

40

100

' I TIM

Environment: Dry Argon; R.T.

- Environment: Lab Air; R.T

-2

10

10

10

o^io-

10

10
10

10
10

10
10
'

10
4

10

40

I I III

100

0.0662
0.158
0.347
0.685
1.23
2.02
3.08
7.57
7.68

9.
10.
13.
13.07 (max)

Life Prediction Ratio Summary


A-E o
i

0.

.5

r-

.8

100

1.25

da/dN (10"6in/cycle)
0.0860

5.83 (min)
6.
7.
8.
9.
10.
13.
13.02 (max)

0.0501

6.
7.
8.

RMS %
Error
11.37

AK (KsiVin)

da/dN (10-6in/cycle)

3.69 (min)
4.
5.

I I 11 ll

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'

10

RMS %
Error
18.25

Figure 6.11.3.1.6
6-124

0.0875
0.110
0.163
0.271
0.490
1.73
1.73

Life Prediction Ratio Summary


en A
-r-

0.

.8

1.25

H Ti-5AI-2.5Sn h
Condition/Ht: ANNEALED
Form: 0.08 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: TL
Stress Ratio: 0.67
Frequency: 54.2 - 58.3 Hz
(3 of 4)

AK (MPaVin)
10

E i
-2

' I 'I'l'l

40

Yield Strength: 125.4 ksi


Ult. Strength: 133.9 - 135.2 ksi
Specimen Thk: 0.083 - 0.085 in.
Specimen Width: 2.753 - 2.757 in
Ref: 88911

100

' I M'l'l

Environment: Distilled Water;


_ R.T.

40
|

4)

100

| l|l|l|

-L

10
10

10

10

10

^10"
\
,_
c
_

_a>
o

^r:

10

o
o10"

o
\

-3 |

10

10
-

T3

x>

SB

-7

10

1 , 1,1,1,

~ 1 , 1,1,1,

40

10

II I I

10

I , I, I,I,

10

100

.8

1.25

da/dN (10"6in/cycle)

AK (KsiVin)

0.395
0.698
3.65
9.00
11.0
11.6
12.5
16.4

4.23 (min)

5.
6.
7.
8.
9.
10.
12.91 (max)

Life Prediction Ratio Summary


.5

100

AK (KsiVin)

0.237
0.362
0.657
1.13
1.81
2.70
3.74
6.70

4.28 (min)
5.
6.
7.
8.
9.
10.
12.74 (max)

40

10

da/dN (10"6in/cycle)

AK (KsiVin)

10

10

AK (KsiVin)

0.

10

10

RMS %
Error
7.18

--o
10

n)

_c

10

10
"~""

io"2

10

.-a
10

_c

10

10

| <|l|l|

10
Environment: 3.5ss NaCI; R.T. -=

10
-

10

"D

(4

AK (MPaVin)

RMS %
Error
30.21

Life Prediction Ratio Summary


Q-CD

0.

Figure 6.11.3.1.6 (Concluded)


6-125

r-

r~

.5

.8

1.25

2.

Ti-6-2-2-2-2

i^i^y^^i

**

:\?:'*o
r-t

1
.5

to
50

T
00

liil

O
1

o
sa;

s
CO

00

CO

as

tt>

t-

CD

ill
ili
*

CO

*r
o

*S

S
0
tf

<y^

eq

CD
^

;>''

"H

^H

'-,

&

Bg

'

PH

W
hH

Sa.

3a.

to

to

K|:!}:

III

fitlliiiii

P
<

llll

:Z
;^w

ill
iil!

ttjss;

ifilSIlil
pilii
:*:*>:*:
ir* >

o
1
X

6-126

Ti-6-2-2-2-2

CM

**mt:>

:::*:::'::&
O

c-

V
I
00

CO
-H
*T

t-

lO

00

/~s

<

H
H
Z
H

1
illil

lilil
o

it
pill
>

p ill

to

CD

.-H
CD

CO
CO
CO

b
5

'

fc^

*a

::-:::::::::::::::

&~

J2 N

pi
S >~'

CD

-i-i-i-l-ivS

-H.r : :

Bs
a

w
a.

lii^Pilll
&*

<

H
Z
H
HH

SftSiW:

NH

lii^iii
lpiii
t"l >"'"

a*3

CO

6-127

Ti-6-2-2-2-2

s
2>

tf

sis
US

tsl-

03
IS

1*5*

9
u

z
2

I
ei
CO

EH

[H

EH

EO

(a

C
GO
04

9PS

S3 K

fe o

E-

EH

.1

EH

E"

S
Q
0

lb

z
o

<
s

o
u

6-128

This page intentionally left blank

6-129

EF

I Ti-6-2-2-2-2
Condition/Ht: ST
Form: 0.63 in. Plate
Specimen Type: CT
Orientation: LT
Stress Ratio: 0.1

Yield Strength: 157 ksi


Ult. Strength:
Specimen Thk: 0.151 - 0.152 in.
Specimen Width: 3 in.
Ref: 86844
(1 of 4)

AK (MPaVin)
4

10

El ' I 'I'l'l

40

100
1

I ' I M'l'l

10

Environment: H.H.A.; R.T.;


_ Frequency: 1. Hz

(2 of 4)

AK (MPaVin)

-2

4
P=-ir-r-r-

10

Pl

40

100

1 ' I M'l'l

10

10

10

10
-3

-3

10

10
_a>

io"2

10

u
\

o 10
\
c

10
z: 10
T3

10

10

XI

BJ

10

10

10

-7

10

II I I

10

o
6-10-4

10

10

10~2 P
o

-3 |

-5

T3

10

Environment: H.H.A.; R.T.;


_ Frequency: 20. Hz

10

10

I , LI,I,

.-8

10

10

40

10
4

100

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error
6.93

Life Prediction Ratio Summary


a
I

0.

.5

.8

1.25

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.0855

5.05 (min)
6.
7.
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
50.
56.48 (max)

1.23
1.68
2.36
4.93
8.17
13.6
22.5
35.5
57.1
95.5
285.
788.
3037.
3918.

8.23 (min)
9.
10.
13.
16.
20.
25.
30.
35.
40.
50.
60.
70.
71.40 (max)

10

AK (KsiVin)

2.

RMS %
Error
6.62

Figure 6.12.3.1.1
6-130

0.184
0.355
0.614

0.976
1.45
3.58
6.61
11.4
18.1
26.1
36.6
51.4
105.
154.

Life Prediction Ratio Summary

0.

.5

.8

1.25

Ti-6-2-2-2-2
Condition/Ht: ST
Form: 0.63 in. Plate
Specimen Type: CT
Orientation: L-T
Stress Ratio: 0.1

Yield Strength: 157 ksi


Ult. Strength:
Specimen Thk: 0.151 - 0.152 in.
Specimen Width: 3 in.
Ref: 86844
(3 of 4)

AK (MPaVin)
1

4
CT|

-2

10

40

I I Mill

EF

(4 of 4)

AK (MPaVin)
4

100
_

I M l Ml

10

40

|.|-|

100

| l|l|l|

-L

Environment: 3.5s NaCI; R.T.; 10


Frequency: 20. Hz

- Environment: 3.5 NaCI; R.T.; -=\ 10


_
Frequency: 1. Hz

10

10

10

10

10

10
2

io"

o
\

6^1 o"4
10
10

-z. 10

.."O

10

_J

O-10-4

\
c

-3 |

"O

XI

10

_fi

o
o
\

E
E

10

_*/o
o

10

10

10

-= 10

10

10

10

"

10

10

10
4

10

40

da/dN (10"6in/cycle)

RMS %
Error
21.60

116.

201.
289.
373.
527.
727.
831.

.5

.8

1.25

0.0620
0.0755
0.301
0.749
1.43
2.32

3.89 (min)
4.
5.
6.
7.
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
49.43 (max)

Life Prediction Ratio Summary


i

100

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.596
0.642
0.924
1.38
2.08
6.63
17.6
48.4

6.77 (min)
7.
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
50.
60.
63.48 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , I,I,I,

- I , l.l.l,

100

10

]-

2.

RMS %
Error
9.15

17.1
31.9

54.5
73.6
89.6
109.
193.

Life Prediction Ratio Summary

0.

Figure 6.12.3.1.1 (Concluded)


6-131

3.41
4.67
9.67

.5

.8

1.25

2.

EF

I Ti-6-2-2-2-2
Condition/Ht: STA
Form: 0.63 in. Plate
Specimen Type: CT
Orientation: L-T
Stress Ratio: 0.1

Yield Strength: 157 ksi


Ult. Strength:
Specimen Thk: 0.143 - 0.147 in.
Specimen Width: 3 in.
Ref: 86844
(1 of 4)

AK (MPaVin)
4

- I

10

40

100

' I M'l'l

_ 10

Environment: H.H.A.; R.T.


_
Frequency: 1. Hz

t I

II I M MM

(2 of 4)

AK (MPaVin)

10

40

' I M'l'l

100

' I M'l'l

Environment: H.H.A.; R.T.;


Frequency: 20. Hz

10

10

-i

10

10

o
^10"+

\
10

10
10

T?

10
10

10
10
-8

10

10

40

100

AK (KsiVin)
da/dN (10'6in/cycle)

AK (KsiVin)

RMS %
Error
6.11

0.

.5 .8

1.25

da/dN (10"6in/cycle)

AK (KsiVin)

0.0622
0.166
0.377
0.700
1.14
1.68
2.34
4.87
8.19
13.7
21.1
27.3
32.4
40.3
44.9

8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
41.87 (max)

100

6.
7.

Life Prediction Ratio Summary


i

40

4.13 (min)
5.

0.509
0.813
1.30
1.93
4.69
8.86
17.0
32.8
57.7
96.7
159.
419.
1188.
2082.

7.18 (min)
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
50.
60.
64.83 (max)

10

AK (KsiVin)

2.

RMS %
Error
8.28

Figure 6.12.3.1.2
6-132

Life Prediction Ratio Summary


a
i

0.

.5

.8

1.25

2.

_!
I

Condition/Ht: STA
Form: 0.63 in. Plate
Specimen Type: CT
Orientation: L-T
Stress Ratio: 0.1

4
=I

10

T-l II l|l|

40
1

i i i

(3 of 4)

i i i

_L

O 10

z
-+"
10 \
o

2 10"5

XI

2 10"5

fl

\
o

-5

10
10"7

10~7

! ,!,l,

I , I.LL

10

40

m"8 1

100

da/dN (10"6in/cycle)

I . I,I.I,

I , LI,I,

40

0.

.5

.8

10

-6

10

100

da/dN (10"6in/cycle)

3.64 (min)
4.
5.
6.
7.
8.
9.
10.
13.
16.
20.
20.05 (max)

Life Prediction Ratio Summary


1

cy

AK (KsiVin)

38.5
37.7
75.5
69.3

-5

10

AK (KsiVin)

14.74 (min)
16.
20.
20.37 (max)

"O

rVr

AK (KsiVin)
AK (KsiVin)

10 >
0

fir

~
z

-6

10

J*
^

nj

~ .-*
10

10

10

<o
2

io"

o
~
\
-3|
10 JE

<u
o
o 10

Environment: 3.5 NaCI; R.T.; 10


_ Frequency: 20. Hz
-

la"3

io"2

a>

RMS %
Error
13.97

100

' I ' I M'l

-1

a>

"

40

-1

m"8

10

I ' I ' I 'I'l

10

ID"3

\
D
" -s

100

| 1 | Mil

10

1
'rr

(4 of 4)

AK (MPaVin)

- Environment: 3.5s? NaCI; R.T.; 10


_ Frequency: 1. Hz

10-2

3-2-2-2-.1^

Yield Strength: 157 ksi


Ult. Strength:
Specimen Thk: 0.143 - 0.147 in.
Specimen Width: 3 in.
Ref: 86844

AK (MPaVin)
1

T:
C
I I L

1.25

2.

RMS %
Error
20.69

Life Prediction Ratio Summary

0.

Figure 6.12.3.1.2 (Concluded)


6-133

0.0686
0.126
0.456
1.11
2.10
3.35
4.74
6.14
9.43
11.8
16.9
17.0

.5

.8

1.25

2.

Ti-6-2-4-2

"
45IOH

<

10

Ssisss

IIIlSl

52
gisstes*:

ip

ilfpll
>.

SSSBS-JHS

imi
Illpi

:;::

: : : 'Ji::::

c4

llllii

mzm

m$m

ta

10
N

&*
N

CD

CD

OT
CO

H:^;:;'

sg

op

fc.o

'.&*;..

H
Z
:^x-G3:-:v:v:v:v::-

filll
:

op

M3
H3
>* w

sis

Illplll

3
X

fc.o

o
o

6-134

This page intentionally left blank

6-135

I Ti-6-2-4-2

EF Condition/Ht:

1790F 1HR AC 11 OOF 8HR AC


Form: 2 in. Forging
Specimen Type: CCP (max load specified)
Orientation: CR
Stress Ratio: 0.1

(1 of 3)

AK (MPaVin)
4

- I

10

Yield Strength: 139.4 - 140.9 ksi


Ult. Strength: 151.6 - 152.3 ksi
Specimen Thk: 0.073 - 0.083 in.
Specimen Width: 1.75 in.
Ref: PW002

40
100
Ti I i I >|i|

' I M'l'l

Environment: Lab Air; 80F;


_
Frequency: 0.16 Hz

-=j

(2 of 3)

AK (MPaVin)
10
i i nil

40

100

' I M'l'l

Environment: Lab Air; 800T;


_
Frequency: 30. Hz

10

-=\ 10

10

10
10

-3

10

10

_0J

<u

5^10-4

5*10"+

-3 |

10
10

z:

Z. 10
x>

tz

x>
10 '\
o

o
x>

XI

10

10
10
-7

10

10

10
I I i I Hi
4
10

10

10

i i

40

100

AK (KsiVin)

RMS %
Error
6.12

10.00
25.2

Life Prediction Ratio Summary


i

0.

.5

1-i

.8

1.25

100

0.254
0.262
0.397
0.515
0.653
0.858
1.19
3.20
5.89
10.1

4.95 (min)
5.
6.
7.
8.
9.
10.
13.
16.
18.28 (max)

1.98
2.42
4.96

11.61 (min)
13.
16.
20.
24.68 (max)

40

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

10

AK (KsiVin)

RMS %
Error
2.06

Figure 6.13.3.1.1
6-136

Life Prediction Ratio Summary


0.

.5

.8

1.25

Ti-6-2-4-2
Condition/Ht: 1790F 1HR AC 11 OOF 8HR AC
Form: 2 in. Forging
Specimen Type: CCP (max load specified)
Orientation: CR
Stress Ratio: 0.1

= I

10

' I 'I'l'l

Yield Strength: 139.4 - 140.9 ksi


Ult. Strength: 151.6 - 152.3 ksi
Specimen Thk: 0.073 - 0.083 in.
Specimen Width: 1.75 in.
Ref: PW002

(3 of 3)

AK (MPaVin)

EF

AK (MPaVin)
1

40
100
Ti I i I i|i|

10

b I ' I 'I'l'l

- Environment: Lab Air; 1000T; ^j 10


_
Frequency: 30. Hz

40

100

1 ' I 'I'l'l

10

-2

10

-1

10

10

io"2

o
_
0-10-4
_c

_
10

10

-5

-ho \
-a

10
-5

~=\
10

10

-6

10
10
4

10

40

'

Li

da/dN (10"6in/cycle)

6.
7.
8.
9.
10.
13.
16.
18.45 (max)

r~

100

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


0.

40

0.680
0.858
1.14
1.42
1.75
2.19
4.50
8.31
16.6

5.44 (min)

RMS %
Error
2.85

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

' i i im

I I 11II

100

.5

.8

RMS %
Error

Life Prediction Ratio Summary


i

0.

1.25

Figure 6.13.3.1.1 (Concluded)


6-137

.5

r-

.8

1.25

EF

I Ti-6-2-4-2 I
Condition/Ht: 1790F 1HR AC 11 OOF 8HR AC
Form: 2 in. Forging
Specimen Type: CCP (max load specified)
Orientation: C-R
Stress Ratio: 0.5

(1 of 3)

AK (MPaVin)
4
10
I I I I Mil

Yield Strength: 139.4 - 140.9 ksi


Ult. Strength: 151.6 - 152.3 ksi
Specimen Thk: 0.074 - 0.082 in.
Specimen Width: 1.75 in.
Ref: PW002

40
100
1I I I I MM

Environment: Lab Air; 80T;


_
Frequency: 0.16 Hz

(2 of 3)

AK (MPaVin)
-

-=q 0

10

40

I I ll.lll

100

. I,,,,,,

_.

Environment: Lab Air; 800T;


_ Frequency: Unspecified

10

10
-1

10

10

10

10
2

CJ

CJ

^10"4

6-10-4
-3 |

10

10"

2 10

10
10

m" ^
u
-o

10

10
-5

10

10

-7

10

10

10

10

10

10
4

10

40

-8

100

7.60

0.

.8

100

1.25

4.87
4.90
5.88
7.76
11.4
22.6
25.6

8.97 (min)
9.
10.
13.
16.
20.
22.81 (max)

Life Prediction Ratio Summary


.5

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.466
0.951
1.58
2.30
5.37
11.4
14.8

7.05 (min)
8.
9.
10.
13.
16.
19.52 (max)

10

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

I , I,I.I.

" I , I,I,I,

AK (KsiVin)

RMS %
Error

I
z

iw

XI

a?

-= 10" o
o
\

RMS %
Error
4.99

Figure 6.13.3.1.2
6-138

Life Prediction Ratio Summary


i

0.

.5 .8

1.25

Ti-6-2-4-2
Condition/Ht: 1790F 1HR AC 11 OOF 8HR AC
Form: 2 in. Forging
Specimen Type: CCP (max load specified)
Orientation: CR
Stress Ratio: 0.5

4
10
I I llllll

AK (MPaVin)
4

40
100
I I illlll
-1

Yield Strength: 139.4 - 140.9 ksi


Ult. Strength: 151.6 - 152.3 ksi
Specimen Thk: 0.074 - 0.082 in.
Specimen Width: 1.75 in.
Ref: PW002

(3 of 3)

AK (MPaVin)

10

40

100
3

= I ' I Tl'lI ' I Tl'l

Environment: Lab Air; 1000T;


_ Frequency: 0.16 Hz

10

10

10

10

o^o"4
c
_

2 10

-o

o
\
-3 |
10 E
-

tz

10

10

10

"

10

io"2^
o
o 10
c

-3 I

10

I , I,I,I,

I , LI,I,

40

10

- io \
D
-u
10

10
-6
10
-

10
10
10
10
4

100

AK (KsiVin)

Life Prediction Ratio Summary


i

0.

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

3.57
4.23
5.58
6.62
7.60
8.74
14.3
20.6
29.7
30.2

5.60 (min)
6.
7.
8.
9.
10.
13.
16.
20.
20.12 (max)

RMS %
Error
4.46

10

AK (KsiVin)

da/dN (10'6in/cycle)

AK (KsiVin)

z: io

ior\
o

idJr

10

10

EF

.5

RMS %
Error

.8

Life Prediction Ratio Summary

0.

1.25

Figure 6.13.3.1.2 (Concluded)


6-139

.5

.8

1.25

EF

I Ti-6-2-4-2 I
Condition/Ht: 1790F 1HR AC 11 OOF 8HR AC
Form: 2 in. Forging
Specimen Type: CCP (max load specified)
Orientation: C-R
Stress Ratio: 0.7

(1 Of 1)

AK (MPaVin)
4

1
I

10

Yield Strength: 135.5 - 140.9 ksi


Ult. Strength: 148.5 - 152.3 ksi
Specimen Thk: 0.08 - 0.081 in.
Specimen Width: 1.75 in.
Ref: PW002

AK (MPaVin)
1

40
100
1M M MM

I I I IMI

- Environment: Lab Air; 800T;


_ Frequency: 0.16 Hz

= I

10

' I 'I'l'l

40

100

' I M'l'l

~=\ 1

10

10

10

10

10
-3

IQ"3

10

jo
2

jo
o

IO"
o

<o

2 T;

10"

jo
o

o
4

frlO"

l 0*

10
-5

Z 10

10

10

Jio >

"o

"O

10

T3

_R
10
10

10
10

10

10

10
.-8

10

10

I I I I 111

I I 11II

10

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

40

100

da/dN (10-6in/cycle)

AK (KsiVin)

1.36
2.04
2.71
3.36
4.16
5.35
15.5
16.0

5.15 (min)
6.
7.
8.
9.
10.
13.
13.08 (max)

Life Prediction Ratio Summary

RMS %
Error

-I-

0.

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
14.63

.5

.8

1.25

Life Prediction Ratio Summary


0.

2.

Figure 6.13.3.1.3
6-140

.5

.8

1.25

2.

Ti-6-2-4-2

S&

O
~

o
o

iS

o
o

CO

3
a

H
Z

s
z

CD
CO

. .. "W.

ft*

uto

o
3

ti

;o^..is N

03

a>

CO
CO

BS
H

Z
0
hH
H
<
H
Z
W
NH

P*

:.

V Z:;
-:H

S :
iftii
:)-< 2 :.' .

<

XH

to

o
ZH

3
Z

^
K

6-141

Ti-6-2-4-2 ELI

iS:
~*
o
o
W&-/-S '

IlliSI

a
0

5*

S
z
o

fllil itii
m
o

IIII

8;*

si::

fiiiii
IIIIIII

O
to

tf

rg
w

CD

1C

cy^
M N
fr.

ffl
;

tf

lllllll
O M '

CD

iiiiiii
A

HI

Z-:

PPIis

w
H4

III S
jgi^j
lllill
mmm$:

111

0H

:*:

0.

llll:

14
O
h-l
<

IS
:*:-:-:j:i:-:i

:?:*:**

^<

<
aH
^
O
to

i
III

z
$

ffl

6-142

This page intentionally left blank

6-143

EF

I Ti-6-2-4-2 ELI h
Condition/Ht: ANNEAL 1450F 1HR AC
Form: 0.75 in. Plate
Specimen Type: CT
Orientation: L-T
Stress Ratio: 0.1

(1 of 1)

AK (MPaVn)
4
_

-2

, |

10

40

T|-j

i |

Yield Strength: 140 ksi


Ult. Strength: 149 ksi
Specimen Thk: 0.187 in.
Specimen Width: 1.5 in.
Ref: MA016

AK (MPaVin)
1

100
jiM|

Environment: Vacuum; R.T.;


Frequency: 9. Hz

- I

' I M'l'l

10

10

-3

10

""""

io"2

io" "

o 10

"O

100

10

10

"*"*

Z. 10
-o
\
o

' I M'l'l

40

10

10

10

10

J2
o

10

-6

10

^10"*
\
c
_

-3l

10

10

10

10 \
o

"o

_,;
10
10

10

:
10

10

-6

10

10
10

i , iiUi

I , LU,

40

10

.-8

10

100

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)

15.85

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.825
2.89
6.63
13.3
31.5
60.9

13.18 (min)
16.
20.
25.
30.
32.99 (max)

RMS %
Error

10

AK (KsiVin)

Life Prediction Ratio Summary

RMS %
Error

Life Prediction Ratio Summary


i

.5

.8

1.25

0.

2.

Figure 6.14.3.1.1
6-144

.5

.8

1.25

This page intentionally left blank

6-145

^ Ti-6-2-4-2 ELI I
Condition/Ht: ANNEAL 1450F 1HR AC
Form: 0.75 in. Plate
Specimen Type: CCP (max load specified)
Orientation: L-T
Frequency: 0. Hz
Environment: LAB AIR;1000F
(1 of 3)

AK (MPaVin)
4
10
40 100
_

I | l|l|l|

I | i|T|

Stress Ratio: -0.3

Yield Strength: 78 ksi


Ult. Strength: 96 ksi
Specimen Thk: 0.187 in.
Specimen Width: 3 in.
Ref: MA016

- I

-i

-=

10
10

ro"
o

o 10

-3 IE

10

10

10

10

10

10

-z:

io"2"

,o-I

_*X>

10

XI

10

"""*

10

10

10

-I

Stress Ratio: 0.02

o
S-10-4
\
c
_

-6

10

100

' I 'I'l'l

~~

40

10

10

"

10

I I >lllll

10
-1

_a>
o

(2 of 3)

AK (MPaVin)

I , I,I,I,

40

10

^z 10

10

I , I,I,I,

10

" I , I,I,I,
4

100

da/dN (10"6in/cycle)

0.

.5

.8

100

0.0740
0.0406
0.0698
0.198
0.244

31.31 (min)
35.
40.
50.
51.13 (max)

Life Prediction Ratio Summary


i

40

da/dN (I0"6in/cycle)

AK (KsiVin)

0.0599
0.0625
0.0637

27.03 (min)
30.
33.72 (max)

RMS %
Error
19.14

I , LI,I,

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

10

t
-

1.25

2.

RMS %
Error
14.31

Figure 6.14.3.1.2
6-146

Life Prediction Ratio Summary

0.

.5

.8

1.25

2.

H TI-6-2-4-2 ELI
Condition/Ht: ANNEAL 1450F 1HR AC
Form: 0.75 in. Plate
Specimen Type: CCP (max load specified)
Orientation: LT
Frequency: 0. Hz
Environment: LAB AIR;1000F

10

Yield Strength: 78 ksi


Ult. Strength: 96 ksi
Specimen Thk: 0.187 in.
Specimen Width: 3 in.
Ref: MA016

(3 of 3)

AK (MPaVin)

AK (MPaVin)
1

40
100
ni l i I i|i|

I- I ' I Tl'l

10

40

- I i I UM'I

100

' I M'l'l

10

10

__

10

-_

10

10

10

z 10"
2

-S2

G-10-4
=
\
c
_

o 10

_c

-1
10

10

Stress Ratio: 0.5

10

-5

Z. 10

Z 10

"o

XI

10

10"

4
N

~'

_e
10

z.

i"

'\
u
-o

~""
10

10

10

10

10
' i i i in

I I iI Hi

10

40 100

10

100

da/dN (I0"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


0.

40

0.114
0.256
0.745

31.38 (min)
35.
38.06 (max)

10

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

1 , 1,1,1,

~ \ , 1,1,1,

AK (KsiVin)

RMS %
Error
15.14

o
\

-J10 >

10

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


i

0.

2.

Figure 6.14.3.1.2 (Concluded)


6-147

.5

1i

.8

1.25

2.

\ Ti-6-2-4-2. ELI I
Condition/Ht: ANNEAL 1450F 1HR AC
Form: 0.75 in. Plate
Specimen Type: CCP (max load specified)
Orientation: LT
Frequency: 9 Hz
Environment: LAB AIR; RT
(1 of 3)

AK (MPaVin)
4

- I

10

I I ipl'l

40

Yield Strength: 140 ksi


Ult. Strength: 149 ksi
Specimen Thk: 0.187 in.
Specimen Width: 3 in.
Ref: MA016

100

' I 'I'l'l

-"

- Stress Ratio: -0.3

(2 of 3)

AK (MPaVin)

~=

10

40

| IM|I,

100

, ,,.,,,

-.

Stress Ratio: 0.1

10

~~*

io"2^

10

-2

10

10
10

:
10
_Q5

10

S2.

2 u

io"

10

_0)

o
0-10-4

6^10"
\
c

-3|
E

2 10
-a

2 10"5

tz
""~*

T3

10T \
o
-o

10

10

-=

10
10

_*-a
10

10

10

tZ.

10

10

-3IE

~ I , l.l.l,
4

, I,I,I,

10

40

10

100

da/dN (10"6in/cycle)

13.
16.
20.
25.
25.15 (max)

.5

.8

100

1.25

1.52
2.05
6.09
13.5
34.2
48.3

12.17 (min)
13.
16.
20.
25.
26.03 (max)

Life Prediction Ratio Summary


0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

4.93
5.61
13.2
21.3
40.9
42.0

12.73 (min)

RMS %
Error
18.34

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , i . I.I.

" I , !,I,L
4

10

2.

RMS %
Error
12.45

Figure 6.14.3.1.3
6-148

Life Prediction Ratio Summary


a
i

0.

.5

.8

1.25

2.

Ti-6-2-4-2 ELI
Condition/Ht: ANNEAL 1450F 1HR AC
Form: 0.75 in. Plate
Specimen Type: CCP (max load specified)
Orientation: LT
Frequency: 9 Hz
Environment: LAB AIR; RT

10

t I ' I Tl'l

40

Stress Ratio: 0.5

I1

Yield Strength: 140 ksi


Ult. Strength: 149 ksi
Specimen Thk: 0.187 in.
Specimen Width: 3 in.
Ref: MA016

(3 of 3)

AK (MPaVin)

AK (MPaVin)
4

100

10

40

VY

' I M'l'l=*

10

100

' I 'I'll

10

10

10

10

10
-3

10

10

io"2

>^.
o 10-r*

O-10-4

10
x>

o
\

10

10

_K
10

XI

10
-5

10

10
-7

10

10

10

10
i I i I Hi

10

'

10

10

i i 11 ii

40

'

I I till

100

da/dN (I0"6in/cycle)

AK (KsiVin)
11.92 (min)
13.
21.13 (max)

100

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


i

40

2.52
6.79
16.9
43.6
57.2

16.
20.

0.

I I III

10

AK (KsiVin)

AK (KsiVin)

RMS S
Error
10.59

10

10
10

"o

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


i

0.

2.

Figure 6.14.3.1.3 (Concluded)


6-149

.5

.8

1.25

2.

Tj_6_2-4-2

ELI I

Condition/Ht: ANNEAL 1450F 1HR AC


Form: 0.75 in. Plate
Specimen Type: CCP (max load specified)
Orientation: LT
Stress Ratio: 0.02
Environment: LAB AIR;1000F
(1 of 3)

AK (MPaVin)
1

- I

10

' I M'l'l

Yield Strength: 78 ksi


Ult. Strength: 96 ksi
Specimen Thk: 0.187 in.
Specimen Width: 3 - 3.002 in.
Ref: MA016

40
100
-ii i i HIM

- I

10

Frequency: 0.25 Hz

(2 of 3)

AK (MPaVin)
10

' I M'l'l

40

100

' I M'l'l

-1

Frequency: 2.75 Hz

10

10

- 10_J E

10

10
10
-3

10

10

io"
o

o^10-4

fri O-

-3 |

10

10

Z 10
10

1^

XI

X)

10

10

_*xs
10 o
-o
10

10

10

10

10

10

10

10
4

10

40

100

0.

.5

.8

1-

1.25

100

3.35
3.56
5.78
8.54
12.4

9.66 (min)
10.
13.
16.
20.
25.
30.
35.
40.
45.26 (max)

Life Prediction Ratio Summary


i

40

da/dN (10"6in/cycle)

AK (KsiVin)

8.44
8.46
11.6
22.8
44.9
79.5
123.
158.

15.33 (min)
16.
20.
25.
30.
35.
40.
43.90 (max)

10

AK (KsiVin)

da/dN (10-6in/cycle)

AK (KsiVin)

1 , 1,1,1,

" 1 , 1,1,1,

AK (KsiVin)

RMS %
Error
15.34

2.

RMS %
Error
7.50

Figure 6.14.3.1.4
6-150

16.9
21.7
27.7
35.8
41.5

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

\ Ti-6-2-4-2 ELI h
Condition/Ht: ANNEAL 1450F 1HR AC
Form: 0.75 in. Plate
Specimen Type: CCP (max load specified)
Orientation: LT
Stress Ratio: 0.02
Environment: LAB AIR;1000F

10

40
i

= I ' I 'IT

Yield Strength: 78 ksi


Ult. Strength: 96 ksi
Specimen Thk: 0.187 in.
Specimen Width: 3 - 3.002 in.
Ref: MA016

(3 of 3)

AK (MPaVin)

AK (MPaVin)
4

100

- I

l i l H

10

' I 'I'l'l

40

100

' I M'l'l

Frequency: 6. Hz
10
10

10
o

o
o 10

\
-3 |

10

-Z. 10
10

-o

X)

_K 10
10
10
10

10
4

10

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

100

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


a o
0.

40

2.55
2.90
5.64
13.2
25.9
45.7
97.3
104.

12.06 (min)
13.
16.
20.
25.
30.
35.
35.37 (max)

RMS %
Error
13.42

10

AK (KsiVin)

AK (KsiVin)

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


i

0.

2.

Figure 6.14.3.1.4 (Concluded)


6-151

.5

.8

1.25

EF

Ti-6-2-4-2 ELI I
Condition/Ht: ANNEAL 1450F 1HR AC
Form: 0.75 in. Plate
Specimen Type: CCP (max load specified)
Orientation: L-T
Stress Ratio: 0.02

(1

AK (MPaVin)
1

4
|i

10

Yield Strength: 95 ksi


Ult. Strength: 109 ksi
Specimen Thk: 0.187 in.
Specimen Width: 3.001 in.
Ref: MA016

AK (MPaVin)

| i |i|i|

Environment: Lab Air; 700F;


_
Frequency: 6. Hz

40
100
i I i MI'I

10

-Ml 'I'll
10

40

100

1 ' 1 'l'l'l

10

io"2

10"

-1

10

10

io"3

10"

-Jio" ^

O10"

o
o 10

-3 |

10

a?

io"2

/\

Z10

-I

io 3 ^E

~~

2:

^10"5

,_
10

\
o
"

10

-a

-6
10
-5

10

10

10"7

10

-6

10

10
10

-B

i i i nil
4

'

10

10

I I I III

40

100

1 ,1,1,1,

1 ,1.1,1,

40

da/dN (10"6in/cycle)

35.5

Life Prediction Ratio Summary


a

RMS s
Error

-r-

0.

da/dN (10'6in/cycle)

AK (KsiVin)

0.712
0.758
4.20
9.90
17.8

12.93 (min)
13.
16.
20.
25.
29.36 (max)

RMS %
Error
17.14

100

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

.8

1.25

Life Prediction Ratio Summary


0.

2.

Figure 6.14.3.1.5
6-152

.5

.8

1.25

Ti-6-2-4-2 ELI
Condition/Ht: ANNEAL 1450F 1HR AC
Form: 0.75 in. Plate
Specimen Type: CCP (max load specified)
Orientation: L-T
Stress Ratio: 0.5

4
t=~~lI

-2

10

40
I

I 11 i 111

Yield Strength: 78 ksi


Ult. Strength: 96 ksi
Specimen Thk: 0.187 in.
Specimen Width: 3 in.
Ref: MA016

(1 of 1)

AK (MPaVin)

EF

AK (MPaVin)
1

100

10

40

100
3

= I ' I Tl'lI ' I Tl'l

I I I MH

10

Environment: Lab Air; 1000T; -=j 10


_
Frequency: 8. Hz
10

10

10

10

10

10

.2?

o
^10"+

^10"4
10

10

10

10
L"0

10

10

"O

10

_.

10

10

10
10

10
I

I I 11 ll

I . I.I.I.

10

40

10

100

da/dN (10"6in/cycle)

AK (KsiVin)

10

40

100

AK (KsiVin)

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

7.49
9.45
31.5
50.7
83.3

14.36 (min)
16.
20.
25.
28.61 (max)

RMS %
Error
14.59

10
10

10

Life Prediction Ratio Summary


a
i

.5 .8

RMS %
Error

Life Prediction Ratio Summary

1.25

0.

2.

Figure 6.14.3.1.6
6-153

.5

.8

1.25

2.

Ti-6-2-4-6

CM

o
o
;:&**

SSOH

SiK?5

3a

Hi

fr

lim

3r

.'

Oi

SiSlKggS

lipfi

lift
<

P
..fa-.

:-:

:-o
3

0*~
N

N
1-1

:1s5 ;
''H

2
O

;:. g . :V.
5SS
o
o

35

HI
H
Z

5
OS

s
** W

III
jS;:^:

111
:;$j::;:

III

Q5

a
a

E
u
a.
en
Z

ZH

OfH

:#-:SK

:::::;::;:

6-154

Ti-6-2-4-6

o
cJ

:*::*>

O
H

/s

4!

&H

3
CG

ffi

fa

**.

z
o
D

1-4

*
J

fa

Z ligi

CO
CO

CO

^)

EH

IS

fa

O
CO fa

fa

c?^

ifaiSiiii

CO

P3

10
rH
CO

fa

faO

zo

WH
:

^\::':"

H ?

O
2

1
S
op
gfa : :

fa*?

A*

:*:*:*:

z
o

WM

<

AH
ipfaiiii

fa

OS

|^

NH

g
o
t

III*!
.:'''

2X
00

o
o
'::::$::

ZJ
or

to

cs

"* -#<

lill

i
ZH
ilipiiiti

o
us

HI

b.
o
CO

6-155

\ Ti-6-2-4-6 h~
Condition/Ht:
Form: Extrusion
Specimen Type: CT
Orientation: LT
Frequency: 20 Hz
Environment: LAB AIR; RT

Yield Strength: 147.2 ksi


Ult. Strength: 159.1 ksi
Specimen Thk: 0.3 in.
Specimen Width: 1.4 in.
Ref: UD001
(1 Of 1)

AK (MPaVin)
4

10

AK (MPaVin)
4
10
E=li I i I Mi
TT

40
100
i I i I MM

= I ' I 'I'l'

40
100
I I I I Ml

VY

Stress Ratio: 0.1


-2

10

10

10

10
-3

-3

10

10

jo
10~2

JO

o
o 10

-3 |

10

10

10

T3

Jio >

10

10

10
10

10

10

10

10
4

10

40

100

100

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (10_6in/cycle)
0.193
0.286

7.20 (min)
8.
9.
10.
13.
16.
20.
25.
30.
33.04 (max)

RMS %
Error
22.40

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i i i MI

i i 11in
4
10

0.486
0.816
2.73
5.12
9.45
23.3
44.6
70.8

Life Prediction Ratio Summary

RMS %
Error

Life Prediction Ratio Summary


1

.5

.8

.5 .8

1.25

Figure 6.15.3.1.1
6-156

1.25

This page intentionally left blank

6-157

Ti-6-2-4-6 I
Condition/Ht:
Form: Extrusion
Specimen Type: CT
Orientation: LT
Frequency: 20 Hz
Environment: LAB AIR;800F
(1 of 4)

AK (MPaVin)
1

10

Yield Strength: 147.2 ksi


Ult. Strength: 159.1 ksi
Specimen Thk: 0.3 in.
Specimen Width: 1.4 in.
Ref: UD001

4
10
i i 11'|'|

40
100
i I i I i|i|

= I ' I ' IT

(2 of 4)

AK (MPaVin)
40
100
1i i > urn

Stress Ratio: 0.1


10

IQ"3
O

o 10

10
-o
10

-7

10

10
4

10

40

100

da/dN (I0"6in/cycle)

AK (KsiVin)

RMS %
Error
8.76

.5

.8

100

0.623
0.741
1.01
1.31
1.66
2.07
3.85
6.87
12.8

5.52 (min)
6.
7.
8.
9.
10.
13.
16.
20.
25.
30.
35.
35.34 (max)

Life Prediction Ratio Summary


0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

1.09
1.16
1.66
3.31
5.41
10.2
17.6
23.2
33.7

8.87 (min)
9.
10.
13.
16.
20.
25.
30.
33.38 (max)

10

AK (KsiVin)

AK (KsiVin)

1.25

RMS %
Error
7.55

Figure 6.15.3.1.2
6-158

21.9
36.6
56.1
57.3

Life Prediction Ratio Summary


i

.5

.8

1.25

H Ti-6-2-4-6
Condition/Ht:
Form: Extrusion
Specimen Type: CT
Orientation: LT
Frequency: 20 Hz
Environment: LAB AIR;800F

Yield Strength: 147.2 ksi


Ult. Strength: 159.1 ksi
Specimen Thk: 0.3 in.
Specimen Width: 1.4 in.
Ref: UD001
(3 of 4)

AK (MPaVin)
4

^ I

10

' I 'ITI

40
100
"Ii
I
i
I
i|i|
I

Stress Ratio: 0.5

(4 of 4)

AK (MPaVin)
1

10

40
100
1i I i MM

i- I ' I Tl'l
10

-2

10

10
10

10
10

10
2

10"
o
6^10"

_Q)

-J10-&

o 10
10

10

-5

10

zn

Stress Ratio: 0.7

10

T3

X)

-A~0

10

"O

10

J10 >
T3

_c

10

10

-5

10

10
10

10

10

10

10

'

I i I ih

10

10

[Mill

40

'

1.35
1.78
2.31
3.01

6.52
10.7
17.8

.5

.8

100

1.25

0.784
0.798
0.995
1.32
1.80
2.48
3.42
6.74
7.16

4.89 (min)
5.
6.
7.
8.
9.
10.
13.
13.67 (max)

Life Prediction Ratio Summary


0.

i i 11 n

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.814
0.976

5.54 (min)
6.
7.
8.
9.
10.
13.
16.
19.33 (max)

10

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

'

i i 11 ii

100

AK (KsiVin)

RMS %
Error
4.18

RMS %
Error
9.87

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

Figure 6.15.3.1.2 (Concluded)


6-159

2.

\ Ti-6-2-4-6 I
Condition/Ht: 1690F 2HRS AC 1550F 2HRS OQ 11 OOF 8HRS AC
Form: 1.8 - 2.8 in. Forging
Yield Strength: 165.5 - 166 ksi
Specimen Type: CCP (max load specified)
Ult. Strength: 180.8 - 182.3 ksi
Orientation: C-R
Specimen Thk: 0.077 - 0.082 in.
Frequency: 30 Hz
Specimen Width: 1.75 in.
Environment: LAB AIR;800F
Ref: PW002
(1 of 2)

AK (MPaVin)
4

- I

10

I I 'I'l'l

40

100

- I

' I 'l'l'l

"~~

I I 'I'l'l

100
A

' I 'I'l'l

-= 10

~~

-=

10

10

10

10
2

io"

o
6^10-4

\
-3 |

-3 |

10

10

z: 10

Z10-5

Jio
>

10

10
~~"

JJ^

10

10
-7

10

10

10

40

10

10

T>

10

Stress Ratio: 0.1

10

- Stress Ratio: 0.06

(2 of 2)

AK (MPaVin)

" 1 , 1,1,1,
4

-r: 10

10

1 , 1,1,1,

10

40

10

100

da/dN (10"6in/cycle)

RMS %
Error
3.56

0.805
1.08
1.52

2.12
4.00
7.28

.5

.8

100

1.13
1.35
1.83
3.55
7.15
11.4

8.51 (min)
9.
10.
13.
16.
17.28 (max)

Life Prediction Ratio Summary


0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.417
0.603

5.05 (min)
6.
7.
8.
9.
10.
13.
14.76 (max)

10

'I,

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I ,

I , I,hi,

1.25

RMS %
Error
4.35

Figure 6.15.3.1.3
6-160

Life Prediction Ratio Summary


0.

.5

.8

1.25

This page intentionally left blank

6-161

\ Ti-6-2-4-6 I
Condition/Ht: 1690F 2HRS AC 1550F 2HRS OQ 110OF 8HRS AC
Form: 1.8 - 2.8 in. Forging
Yield Strength: 165.5 - 166 ksi
Specimen Type: CCP (max load specified)
Ult. Strength: 180.8 - 182.3 ksi
Orientation: C-R
Specimen Thk: 0.079 - 0.083 in.
Frequency: 0.2 Hz
Specimen Width: 1.75 in.
Environment: LAB AIR;800F
Ref: PW002
(1 of 3)

AK (MPaVin)
4

10

40

100

10

Stress Ratio: 0.1

(2 of 3)

AK (MPaVin)
4
10
- I I I >lll>l
I
Stress Ratio: 0.5

40
100
' I 'I'l'l
-1

-2

10

10

10

10

10
~~

_0>

io' .

o
\

-3 |

10

ZL 10

10"

l_

10"

o
o^10-4
\

-Z. 10

~~

<D

o
\

'I

^-^
Z

m~ ^
o
T7

10

10

10

10

10

10

.-8

10

- i , i .i.i.
4

10

10

i ,i,i,i,

10

40

10

100

da/dN (10'6in/cycle)

100

.5

.8

1.25

3.36
3.77
4.62
9.03
18.1
21.3

8.16 (min)
9.
10.
13.
16.
16.58 (max)

Life Prediction Ratio Summary


0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

4.53
6.74
11.8
18.8
29.7
41.4
69.8

13.03 (min)
16.
20.
25.
30.
35.
39.00 (max)

RMS %
Error
5.05

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

1 , 1,1,1,

" 1 , 1,1,1,

2.

RMS %
Error
2.60

Figure 6.15.3.1.4
6-162

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

Ti-6-2-4-6

Condition/Ht: 1690F 2HRS AC 1550F 2HRS OQ 11 OOF 8HRS AC


Form: 1.8 - 2.8 in. Forging
Yield Strength: 165.5 - 166 ksi
Specimen Type: CCP (max load specified)
Ult. Strength: 180.8 - 182.3 ksi
Orientation: C-R
Specimen Thk: 0.079 - 0.083 in.
Frequency: 0.2 Hz
Specimen Width: 1.75 in.
Environment: LAB AIR;800F
Ref: PW002
(3 of 3)

AK (MPaVin)
4

10

40

- I ' I Tl'l

AK (MPaVin)

I ' I M'l'l

100
"

b I

_L

10

40

' I ' I'll

100

' I 'I'l'l

- Stress Ratio: 0.7


10

10

6^10"

10

.-6

10

10
.-8

10

10
-1

10

10

10

io-2
o
\

zz

ifrr
f
A

o
_
>,,-4
u 10

-3 |
-__ 10 E

10

^10-*^P
\
T3

10

10
=

10
-7

10

10

~zz 10

" I , l,!,l<
4

10

, 1,1,1,
40

10

'

I 111 ill

10

40

100

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

I I 11 ll

100

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

2.46
2.48
2.81
3.43
4.31
5.40
6.71
11.6
14.3

4.73 (min)
5.

6.
7.

8.
9.
10.
13.
14.43 (max)

RMS %
Error
5.36

-z. 10

ior\
=
o

10

Life Prediction Ratio Summary

RMS %
Error

Life Prediction Ratio Summary


i

.5

.8

0.

1.25

Figure 6.15.3.1.4 (Concluded)


6-163

.5

.8

1.25

2.

\ Ti_6_2-4-6 r

Condition/Ht: 1690F 2HRS AC 1550F 2HRS 00 11 OOF 8HRS AC


Form: 2.8 in. Forging
Yield Strength: 166 ksi
Specimen Type: CCP (max load specified)
Ult. Strength: 182.3 ksi
Orientation: C-R
Specimen Thk: 0.08 - 0.081 in.
Frequency: 0.2 Hz
Specimen Width: 1.75 in.
Environment: LAB AIR;600F
Ref: PW002
(1 of 3)

AK (MPaVin)
1

= I

10

' I MM

40
100
i I i I i|i|

(2 of 3)

AK (MPaVin)
- I

10

40

1I

' I M'l'l

100

' I 'I'll

Stress Ratio: 0.5

Stress Ratio: 0.1

10

10
10
10

_a>
o

-^io"2

o 10
10
Z 10
~o
\

o
*

cz

_.T3

10

-el-

10

-5

10
10
10

IAA

10

40

100

RMS %
Error
9.18

Life Prediction Ratio Summary


0.

.5

.8

1.25

1.29
1.48
2.85
3.69
7.34

7.88 (min)
8.
9.
10.
12.83 (max)

2.18
2.30
4.93
9.23
17.0
27.1
40.6

100

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

10.60 (min)
13.
16.
20.
25.
30.
32.52 (max)

111in

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'

i 111in
4
10

10

1~"

2.

RMS %
Error
4.98

Figure 6.15.3.1.5
6-164

Life Prediction Ratio Summary


r-

.5

i-

.8

1.25

2.

1 Ti-6-2-4-6
Condition/Ht: 1690F 2HRS AC 1550F 2HRS OQ 11 OOF 8HRS AC
Form: 2.8 in. Forging
Yield Strength: 166 ksi
Specimen Type: CCP (max load specified)
Ult. Strength: 182.3 ksi
Orientation: C-R
Specimen Thk: 0.08 - 0.081 in.
Frequency: 0.2 Hz
Specimen Width: 1.75 in.
Environment: LAB AIR;600F
Ref: PW002
(3 of 3)

AK (MPaVin)
I-

4
10
' | ' I'l'l

AK (MPaVin)
4

40
100
' | ' HHI

10

40
1

TT

100

I 'I'l'l=>

10

10
10
10

-Jio"2

2
o

5^10-

- 10-J E

Z 10

-AT>

10

-6

10

10
-7

10

10
' i i mi

10
4

10

40

100

da/dN (10"6in/cycle)

da/dN (10"6in/cycle)

AK (KsiVin)

3.68
4.57
12.4

13.3

Life Prediction Ratio Summary


i

0.

100

0.881
1.09
1.60
2.24
2.94

4.41 (min)
5.
6.
7.
8.
9.
10.
13.
13.24 (max)

RMS %
Error
6.37

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

.5

.8

RMS s
Error

Life Prediction Ratio Summary


i

0.

1.25

Figure 6.15.3.1.5 (Concluded)


6-165

.5

.8

1.25

\ Ti-6-2-4-6 I

"

Condition/Ht: 1690F 2HRS AC 1550F 2HRS OQ 11 OOF 8HRS AC


Form: 1.8 in. Forging
Yield Strength: 165.5 ksi
Specimen Type: CCP (max load specified)
Ult. Strength: 180.8 ksi
Orientation: C-R
Specimen Thk: 0.074 in.
Frequency:
Specimen Width: 1.75 in.
Ref: PW002
Environment: LAB AIR;600F
(1 of 1)

AK (MPaVin)
4

^ I

10

' I TIM

40
100
-ii i i i nil

AK (MPaVin)
I-

=q

4
10
i I MM'

40
100
"Ii I ' I'l'l
10

10

Stress ratio: 0.5

-2

10

10

-1

10

10

10

10
-2 T-.

V
O

io"2

O-10-

6^10-4

-3 |

-3 |

10

10

.-s

z. 10

10

10

XI

10

10

10
10

10

10

10
-8

J_J_

10

_U_L
10

40

100

10

I I I III

40

100

AK (KsiVin)

da/dN (10_6in/cycle)

AK (KsiVin)

'

I I llll

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

4.48
7.34
11.9
19.1
30.2
44.5
60.2
110.

13.85 (min)
16.
20.
25.
30.
35.
40.
47.39 (max)

RMS %
Error
6.98

_fi -

10

10

10

Life Prediction Ratio Summary


i

.5

.8

RMS %
Error

Life Prediction Ratio Summary


i

0.

1.25

Figure 6.15.3.1.6
6-166

.5 .8

1.25

i-6-2-4- r

Condition/Ht: 1690F 2HRS AC 1550F 2HRS OQ 110OF 8HRS AC


Yield Strength: 166 ksi
Form: 2.8 in. Forging
Specimen Type: CCP (max load specified)
Ult. Strength: 182.3 ksi
Specimen Thk: 0.079 0.08 in.
Orientation: CR
Specimen Width: 1.75 ir .
Frequency: 0.2 Hz
Ref: PW002
Environment: LAB AIR; RT
(1

AK (MPaVin)
4
10
I ' I ' I' I I
I
Stress Ratio: 0.7

40
100
' I ' I ti

of 1)

AK (MPaVin)
1

-i
0
-= 10

= I

10

I 'ITI

40

100

' I 'ITI

_L

10

io-2

10"2

IQ"3

-1

10

<u

"""x

QJ

-2 T;

10

io"3
""N

<D
O

_c

-^
~

Z10"5

10 \
o

$
sB
B&

-6
10

io-7

XI

/
/&

10
40
AK (KsiVin)

-6
10

-5

-6

10

- I , I,I,I,

m"8
1

I , I , I.I,

10

40

100

AK (KsiVin)

da/dN (I0'6in/cycle)

da/dN (10 "6in/cycle)

AK (KsiVin)

0.00455
0.0109
0.0645
0.135
0.197
0.264
0.546
1.57
4.66
11.9
20.1

Life Prediction Ratio Summary


i

10

100

1.86 (min)
2.
2.5
3.
3.5
4.
5.
6.
7.
8.
8.59 (max)

0.

___ 10-4"
\
*"o
T?
_

10
i I 11111

z:

\
o
~

<D

T;

-1E,

io-7

_2

10
10

-6

AK (KsiVin)

RMS %
Error
24.36

-s
10

~_ f,
f | , |,|,

m"8

zio"5

+ "

i*

"^ 10

_c

10

S^o"4

^10"4

-a
\
o
"

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary

2.

0.

Figure 6.15.3.1.7
6-167

.5

.8

1.25

2.

\ Ti-6-2-4-6 I
Condition/Ht: 1690F 2HRS AC 1550F 2HRS OQ 11 OOF 8HRS AC
Form: 2.8 in. Forging
Yield Strength: 166 ksi
Specimen Type: CCP (max load specified)
Ult. Strength: 182.3 ksi
Orientation: C-R
Specimen Thk: 0.078 - 0.081 in.
Stress Ratio: 0.1
Specimen Width: 1.75 in.
Frequency: 30 Hz
Ref: PW002
(1 of 2)

AK (MPaVin)
4-

10

= I ' I Tl'l

40

100
A

I ' I M'l'l

- I

10

Environment: Lab Air; 80T

(2

AK (MPaVin)
10

'I M'l'l

40

2)

100

' I M'l'l

Environment: Lab Air; 600T

-= 10

-2

10

10

10

10

10
~*

_a>
o

o 10
c

-1

10

"

_a>
o

6^10-4

-3 |

10

_0)

io" ^

10

E^

-5

: 10

.-6

_*-o
10 o

XI

""""*
XI

-ho
>
x>

10

10

10

10

Jp

10

10

10

-z.

10

-6

10

10

.-8

! , I,I,I,

I , I,I,I,

40

10

10

i I i IIh

100

da/dN (I0"6in/cycle)

RMS %
Error
2.66

0.729
0.984
1.40
3.23
6.33
9.10

8.23 (min)
9.
10.
13.
16.
17.43 (max)

0.105
0.186

0.312
0.490
0.723
1.01

2.39
5.80

Life Prediction Ratio Summary


0.

100

da/dN (I0'6in/cycle)

AK (KsiVin)

0.0968

4.87 (min)
5.
6.
7.
8.
9.
10.
13.
14.06 (max)

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

1 , 1,1,1,

10

.5

.8

1.25

I"'

2.

RMS %
Error
1.78

Figure 6.15.3.1.8
6-168

Life Prediction Ratio Summary


0.

.5

.8

1.25

HJ3
CO

'

'

'

CN

CN

CN

i-i

lO

co

CS

0 >

t-

cop
C

e
o

+3

ra

4
sr

e
o

fef

iJ

"o

E*

03 Q

eo

'

1
I

CN

eo

CO

CO

CO

CN

CO

en

to

<*

i-5

Tf

CO

co

CCN

i-H

CO
eo

eo

CO
CN

CN

eo

i-H

03
t~

to
CO

CN
CN

CO

'

CO

CN

CO
CO

CO

CO

1-1

'

CO

Ti-6A1-4V

CO
C-

eo

CN
CN
CO

*>

CO

03

es

"0 1
we

CM

CN

CO

CO

CN
CO

CO
CN

lO
to

00

co

Tj

CO

ei

CN
If

CO
t-

CN

10

i-<

CO

i-H

i-i

CD

w
N3

c
1

00

f<

1-t

i-H

c-

CO

s s

co
CN
CO

o>
U3

cs

H
es

eo

1-1

O
O
H

<

O
CJ
Eh

i-H

fa
lO
c-

fa
fa
o

m
fa
o
g

rH

to
r-l

i-(

d
0

<

<

i-t

ft

a
fa

CN

fa
o

K
33
co

fa
to
t
co

Q
63
J

<

a
S3

fa
u
o
fa

<

OS

fa
s^<
i-H

T-t

o
<
1H

fa

1-H

fa

fa
to
t-

1-H

H
Ed
CO

<
<
<

fa
C3
K

o
CQ

<

O
lO
t-

1-1

-w
0)
eg

fa

&

6-169

<
OS

<

co

CO

Ed

OS

fa

CN

fa

0
*o ois

OS
SB

fa
o

.rf

<

-*
ao

60
C

'P

,o

fa

s<

as
"CP
fa
S
eo
Q

<

T1-6A1-4V

^
02

CN

CO

05

IO
CN

00
IO

CN
CO

0
CO

CO
CO
TT

co

CO

*f.
o

en

'

as a
c

c-

05
CO
00

CO

CO

04

CO

05
CO

IO
CO

i-H

00

CO

,
'

00

.1

05

CN

IO

CO
CO

lo
CO

CN

00

'

IO

to

1-*

CM

CN

OS

eo

CO
05

CO

C05

CO
05

05

IO

CN

o
**
4J

ra

fei
a

e
o

.5

&

i-3
i

CO

Tf

1-H

S
**
o

tf

c-

a?

P
W
P
P

IO
05

<*

CO

if

02

H
l

co

a >

03

C0Q

e
S

CO

'

<*

05
CO

IO
IO

05
O

CO
eo
00

eo

IO

CO

co
CN

IO
eo

00

CO

T(

t-t

'

IO

CO
CO

eo

at

CO
i-i
CO

fa
W

o
o

CO

0)

-w
es

I-H

fa

<
S

CO

Q
Ed
C5

<
OS

p U
fa <
<

fa

Da

H
Ed

<
2

<
2

P
Ed

Q
Ed

O
OS
O

fa
ea

<

K n

<
2

Q
Cd

gcN

TO

1<

o
o

B<
fa
o

H
Q

CN

<

Q
.Ed
3

<

CO
1-*

Ed
O
Ed
OS

22
PS fe
63 fa
05

Q
Ed

OS

<

<

CN

fa
8

CO

<

ae

Cd

QO
Ed H

s<
f
^

fa

ra

**

0 S
^
fe
o o

"?

ESB

P-I

6-170

c
_o

CO

PS

E
X
Ed

+J

ca
o

fa

fa

CO

Et.

Ti-6Ai-4V

CM

ii
*
SSDK
i:*:**::

saos:
''

<
HI

0>:

*-*
a
>

i-H

llflfl

IIII

*3

Z
O

ff~

9
S-

wmmm

CU

CQ

P<

11

S|s3IIil

inpiiii
S"< 5

Z
HH

IgHi Wzm
vK&vX

2S

ZH
illpilll
8
111

6-171

Ti-6A1-4V

<

O
H

...*

'S

02

llill
o

1
it
lllii

H IIII

fa

t>

c-

issiii

Z
fa

0)
*r

is?*

02
02

V)

II

B
02

ft

-*

1-4

Bz
w

1.s

ca

VI

z0s

-*J
e<

tf

02
OH
CO

fa H

CO

fa

,H

"

iH

GO

O
ZO

fa

fa
Q %
>

^lll

I
:-:-:*"*:-::ia::-:-:-:-:-:-:->:-:

III

lilllllt
OH

tn
S

CO

111

14
O
I(
H
5
H
Z
fa
M

i:?:S?

glgg:

H
Z

III:

S1I1I
Aplill
$Mmmmm
ZH
plll!

D
K

3Ed

III

6-172

TJ-6A1-4V

CM

*
si-;;

;:;:;:iwt;:

o
o

/~>

s*

3
fc

&

man

<s
o

<-<

M
^

ClO

t-

e-

'T

CO
CN

CO

/"I.

lilpli
o
:SiaW:*r;:S:

"i
liilll

111
<

fc.

CO

00

CS
TT

to

CD
CO

W5
CO
CS

CD

CO

a
eo

CM

CO

CJ

CD
O

IN

CD

CM

^
CD

CO

CO

z
o
tf

94

QT~

GO

co

CD

co
o

H
ca

ca

Ed

cu

a.

*j
rH

-*

~*

~*

CD

CO

eo

CO

CO

'

'

CD

~*

~*

CO

CD

CO
O

U3

CO

CO

CO

CO

ci

CD

i-H
CO

^S-

&
Z
a

s
H
J

tttllllll

o.

H
ca
w
X
to

a.

SW

o
11

Ipillll

<

W
N"l

<
*

itiPIIl
in
f* 52

S
S
O

<

ca

to
w

u
o
is
a.

CH

US

CD

6-173

<
Q

CD
D

T1-6A1-4V
CN

C-i

::::

' **

:***

PH

O
O

IS

CG
CO

Q
W
Q
P
U
Z
O
U

CO
CO
CD

CD
CO
CD

o
d

CO

co'

CO

co

CO

co
co

CM
CO

CD

CO

CO

co

CO

lllii

PH

Is]

CG

iPlipili
w

CO

CO

CO

CO

es

CD

co

CO
O

CO

co

co

co
o

CO

fe

PV'

o
Zo
P-H

CO

sssssssaes

Z
0

i-H

CO
CO
CO

/-V

CO

PH

c-

t-

3
u

iO

co

CO

o
d

PH

W
Q

SI

>

2
O

QPH
CD

Op

111

PH

:;&::-:?

|:!:j:!:!:i:

*::$:

Io

ti

EL.

IM

<

: z.

< 5*

ii

NH

PH

<

llipiiii III

6-174

Ti-6AI-4V

isss

ssos
*-t

sii??

a>

00
OS

OJ

<r**

ft

llllif
o

:S:SS;:;:Jij;:i:i:;

iilli
P

C4

lip
3
3

GO

P3

ci

_,

-H

^H

ia

s;sj>i:s*i:s;;;

i&i
<j

li.

JO
C4

C?^v
65 iS

iMilil
CO
lH
SO

CO

Sg

E
flliflflllt
s

a.

A*

H
Z

op
" >

: :

S
Ipgili
lisiiii

<

iilpill!

6-175

Tf-AJMV

CM

cJ

SSK
**

us
to
*

:D

/-N

"<#

1
Ills!

-3

H
Z
H

S******
k.^

**.

ML

H is
111!
m&<$m*x

*a

CO
N

ci

ir

to

CO

*""'

""*

CO

CO

CO

Z
0
tf

e*

,,

H
&^

CO

Q
WO
ZO

.;.?.; :;-'V:1

Q
%

o
o

o
o

o
o

.,:K,... '

RODUC
FORM

CO

CO
I

H
J

Z
O

<u
H
Z

w
11

O
Z
OS

a
a

o
Eh

z
5
as

a
a.

A:-.:!. ^

. Z:

III1I
ipi
OS

CO

<
S

ZH

lupin III

6-176

<

T1-6A1-4V
eo
Cw

o
o
SSDK
<-t

SS*!

/">

o
e<i
CN

o
o

3s

llflll
3 in

mm*~m
KHK$*K

SS:::SS::S

IN
O
*H

CO

CO

ci

t00

OJ
CM

CO
CO

00

CO

OJ

CO

CO

CO

c~

00
CO

CM
CO

Cl

4
V

^H

CM

us

to

00

05

O
CO

-**

00

'

c-

o"

CO

*
:l$l:l;::

lllllll

o
*c

o
o

o
o

iO

IO

CO

CO

'

o
C4

O1^
O

O
CO

;|B;

CO

CM

lO

IQ

CO
CD

1
op
S

o
2
n

n
u.

O
b.

2
O

35

P*
1111
H
Z

op
o

g|

HI

!
a
o
OS

H
OH
9-3

<

ffl

<!

CO

<

6-177

T1-6A1-4V
CO
CM

o
<=
o
ft

SSO.

/\

.3

5
H

IO
O

CO

mmm

1
s

io

CO

Iltpll
s

:S:S:!:i:S*iS
S&S8KSK

ill

IjgiJK:
"r

IO
IO
CM

MM

NJ

CO
00
CM
CM
CO

CM

00
cp

-*

CO

~*

C00

CM

IO
CM

CM

-H

CO
C-

CM
CO

IO

-H

CO

IO

*f

wmmm

iiiil

00

o
d

o
co

CM

tt

O1^
fa

CM

o
CM

CM

CM

CM

CM

E-

CM

CM

CO

09
O

00

00

IO

CM

CM

CM

CO
CO

III*

op
H
J

o
hH
H
<

H
Z

ti

CM

CM

CO

2
O

Ed
J
J

to
D

3
ES

111

Ed

Ed

0.

0.

Ed

ft

:::$>:
vX*:*:

1
op

S**!*sSIS

feS

K4S

111

IT-

l
m

''ir':':QS':':*:':':*:':':*:':'::'

ZH

SSS:

OCH

iS:*i

z
%

Si*

6-178

Eh
IO
CO

F-

Q
Ed
Ed

111

<
E0

Ed

U
O

ES
C

<

E-i
Ed
EQ

<
S

CM

to

T1-6A1-4V

05
O

**;

CO

4SS

o
o.

^H

CM

CM

CM

<

CO

IO

CO

IO
IO
CM
CM

CO

W$i&

Si

3
s

GO

a
1

wmm
llipl
llliii

es

CM

CO

CM

CO

IO

CM
CO

CO

ad

o
0

z
o

tf

Q
Q
P
O

C-,
m

z
o

CM

CO

O
CM

CM

CO

CO

Iplllll
-o :..

CO

o
d

PS

go

ittlitllll

Ed

O
2

a.

1o

cs

b.

Ed

Z
O
(-4
H
<
H
Z

h-1

tf

. -.Z

gBi
pi
gs

<

6-179

IO
IO

Q
63

E
O

w
a.

2
3

!Ti-6Ai-4V

o
o

s*?;

<

o.

W3

to

TT

sS>;:

/\

e *

Ulli

*"
';;.:...-

*-*

CO

*r

8
>

'.

st;

rt

v'

o
o

R
U

llfcl

"

|;I

**,"

*
0

w
s*

c^

SB
CD

o
o

o
d

!-3i'i^

Q
>

U
Z

1o

CO
;:

: : ::

;:

o
35
D

S : :S;vw: : : :^: : :KAlflvJ :^

O
H

w
o

SSSftS

Og

SffiSS

':':S-I.-S:'-. *

S3

*#:*:*:

<

<
S

2H
OH

Hl

ffl

6-180

TJ-6A1-4V

::::
O
O

o
o

CO

O
to

03

eq

**

cs
eo

IO
IN

CO*
CO

a
00

1113111
>

:*:!*;**);*;:
w

llpl

*"

ta

CM

Bssi*S;i

c-

e
to

T*

c>

CO

eo

es

es

es

o
00

oo"
CO

CM

o>

c-

^H

es

rr

eo

00

CO

00

*o

[liHlli
o
o

ti

tj

JO
C4

.
H

o*^

JS

cq

B
fe

"?

1-5
CO
1-1

CO

00

00

Ed

E-

co
o

CO

OS

00
o

CO

W3

00

s
i?^:::::,.

*"*i
P

cw

ta

s s
0.

a.

Z
H

HH

CQ

CL.

CG

2S-SS

1
O

0.

Cd

111

::::::

<

ca

2
O

b.
.

V?.
O
N^
H

iiiili
s* 5
<

CQ
Q

6-181

<
s

TI-6A1-4V

-<

::::>

to

T>
7

All .?,

.1"

ft;

CO
CO

KSSSSSRMS

1
es

to

iiiiii
;$m$mg

Illl
:*s5*s;s

mmm

o
1C

o
tf

Q*,-*

ifgfJS

Si

iHliliil

.'g*

'

:OW-a.

en

'
O
HH
H
<
H

HH

iliiiliiii
A<

H
H
^P
rog :.:;.;
f< i*

H3

<

CD

<

cs

ffl

6-182

T1-6A1-4V

o
o

ssos
^K

00

o
e*
o

cU3
lO

cq
C>

es

*>+

0$

C~
CO

CO
CO

CO
CM

ai

CO

CO
CD

io

co

co

<

to

WD

OS
CC

<

ISM
K

3
<

CO

Ol
N

CO

co'

S?*;!!

CO
CO

*
3

2
O

tf

O1^

ar aw

63

63

63

963

co
CO

^*%'^

ta

63

63

a.

cu

a.

2
a
J

::

O
<3

E-<
Z
6J

2
D
ia

hH

*-< 5<

s
lllgiill
liiiiiii

<

<
a:

o
u

963
H

63

S3
63

S3 Z

9 9
a

63

pilll
liiiiiiti

>63

63

63

to
63

CS

to

6-183

63

J
63
K
to

to

T1-6A1-4V

WM

o
o

: JO

:5U
I1S1
O'-;:!

llil

L*5 :

gi s
III

ii

^:

Sll

saos

S
es
CD

foSN

P5

fill
w

6-184

T1-6A1-4V

<d

SS

-*

o
o
(4

0)

IP

53

iititi
o

>

11

**

V)

o
o

Q
iilfcp:
H

CO
<N

IN

C*

CJ

CO

00

t>

W
W

IN

>o

tc

00

~*

~*

-I

00

CO

IN

CO

iiliii
mWmm

ilpi

lO

c4

'V

c^

''

**

'

to

rH

CO

IO

IpIIIII
W$M

igiilSliil
Illlll III
J

ii

PSS

os

CO

a.

0.

fcL.

w
5

9Ed

111

H
<
H

E-i

o
h-1

2
O
CO

Q
&3

' ' Z.V.

ipseplis

l$il

&

Sawi
mfM

5 iis
mm
iililt
m*&Jmm^ *:*:*:*:

Ill

ZH
O fa

3U

<

<:

CO 2

:?SS:*::QS4SS::SS

3
cc

ffi

co
a

ll

CO

CO

6-185


o
SSOK
;:*:

o
o

lpi
b III
3s"
3

z
o

fe

CO

CO

53

Ilf

CM

^
00

IN

CO

eg

CO
CM
CM

i>

CO

CM

CO

IN

CO
CO

c-

CM
CO

CO

CO

CD

0
00

CM

CM

trio

c-

CM
CO
CM

mimm

lliitei:

:j:|:ox*:{:

tf

6
3*

(?.-*

PU

oi

c-

CO

**
>

H 1

CG
CO

0>

SSp^S:;:;:;:;:;:;

mmsm
mmarrfm

Z
H
H
Z
ii

CO

CO

CO

CM
CO
CM

c-

CO
CO
cCM

S:i::^~iS;:S

02

>o

CO

CO

-<

CO

CO

CO

CD

CO

o
d

CO

CO

CO

^-4

CD

CO

U3

"

o
pH

CD

Q
H

CO

O
O

'

'

o
d

CO

00

o
d

CO

o
d

o
d

HI)

>

gg
og

CO
I

Z
Cd

H
Cu

%
a.

to
D
ta

B3
Eg

to

a.

go

63

ft,

H
H
Z
W
M

<

H
.v.-;Z:': :..

&H

siiii
iiilii
irt S3
8-*s

<

ffl

6-186

Ti-6A1-4V

CM

t'3

::>:+:::::

;.-.:

sS>*i

HI

IUI

1
5

i-H
CO

!::;

mi

gs

gg to

111

6-187

Ti-6Al,4Vl

::':o:^:::::$:^:-S-x-

;:|^:;:;:;:^j:^:j:o::

o
o
^

O
H

SK>;

>l

<J

CG

lili

IlfII

::S:::::;j:H:JNj;:::;:

B
z

03
CG

S3

CD

3
H

CO

CO

CO

CO
CN

CD
CO

CO
CO

CO

CO

*2

el

W
ff-.

LEVELS
TEMPE

CO

*r

iiiiiif

z
o

i-H

3
CM

CG

1-5

io

*o
o

fa

OS
HO

'.'"':V;/.

zo
E*
Hh
Q<
H>

*<

g^
H co

op

ill

sill

&x*:S

Z
H
HH

5a.

US

11

<
H

A<

iJ

'

Bs

<^

H
Z

vv:*:;

l;^:S

"-. 111:*:

NH

iZisiiii SSll
paipilil
s^mmmm

<

ZH
III
i^lplffl

6-188

TJ-6A1-4V

CM

SSSJi

ss:;

:.*-*

c-

CO

. to
/-K

*3

iSSS^iSSSS

S*4S^S*

Hill
lllS
iitpt
*<

tlipl

a
o

CO
CO

to

CD

i;#&;s

wm$m

>0

CO

&^
d

~*

CO
CO*

IN

l&Mr:

CO

o
d

O
Z

Cd

ig

1O S

63

EU

b.

fe.

cw

IPI11

D
J

fS:i|5

<
ffl

<OS

om

CQ
K

:Si?:l1?
Ed

to
to

Ed

es

6-189

Ti-6AI-4V
IN
CM

o
SSsS

CO

CO

CO

,-v

J8
tl

3
4a
es

H
S
O

111

H
o

*r

CO

CM

CD

CO

U3

C^

U3

U3
O

**!

CO

CO

CM

CO

CD

U3

&H

SSSSwriiw

SS>fSSSS

llllll
ail
iipi
iliiSil

to
CD

"V

- f"

CM

CM
CO

CO

CM

00

CO

CO

o
d

CO

U3

<1

o
'3

o
d

CM

CM

o
d

o
d

tf

*,-,
0*3

CM

CO

CM

CM

CM

CO
1-1

CP

^^

V
O

CO

CO

*C
O

V
O

CM

CO

a
2

2-

O
2

PQ

2
O

H3

5
o
6-

liiiiliin til
A

D
-1

gW
HH

HI

<

H
Z

mmmm 111

H
2
W

i^ipiii

op
:^Sf:;:p:ii:li!s

Q
U

2
2

o^

<

lit

11111111 $i:S

tu

1
2

SB

ca m
2
O
d N

a
D
W
Q
J
U

Q
W
Q
J

5 5

6-190

<

Ti-6A1-4V
03
CM

::*:::
:*:;
-.-p^

<

O
H

o
o

mmvism

a>

00
0

CO

cw

2
$4

3
1

CO

Z
H
Z

z
CG
CO

&

CO

CO
CO

co

co

c>

2
O
CO

Ed

Z
Ed

Ed

JSS*i3fSSS*

iiilpi
pi
llilil

3:11:

3 zotf

cc

CO

Q
P

o
iH

CO

<y^

B
w

S
HO
ZO

^&"': :

iO

FH

CO

<<?

PS

g3
H co

cs
''"B'-''^^''*-'''-*''''-'^'*'

ij

X
H

0-

a
J
Cd

2
a
Ed

fk .

o
H
<

Z
W
Ft

S3

Q
J
Ed

Z
Cd

2
Ed

o
j

to

. Ed
CO z

Ed

BJ O

Zs
liliillt
<
s

<

ES

...S;
8

Ed

Ed

Ed
ES

Ed
ES
to
to
Ed
CS

to
to

Ed
ES
free

6-191

fr10

Ti-6A1-4V

>sos

O
H

.a

B? IIISl
?
o

iiiiii
III
p

iiiii

Ml
52
is^-ii
lltolSl

CO

O
SS!*:

CO
N

0)

CO

CO

ec

c-

CN

*::?.:;

o
o

IS*
is

Ail
mam

cr~

CO

Hi!
Bill

iH
CO

to

>;:':;:

op
?*.>.

O
2

2
O
t
D

III
' III

X
63

Z
O

z
H

I||
H
Z

ill:

Zg
OB

lii

iKii;
ff 55

::::::

11!

<
CO

<
s

zP

RH
Q< :

;S

6-192

Ti-6A3-4V

o
*sps

tt
<

o
o

iK*SS

ez
cc

C5
rH

cs
CO

VELS OF S
MPERATU

DH H

o
o

I
CM

to

IO

CO

CO

CO

cco

c-

CD

CO

CM

CO
CD

to

to
N

CM

IN

cq

11

c-

c-^

CM

CO

c-

to
CO

to

CM

CM
CO

CO

cc

to
CM

01

H
Z
H

z
o

m$3mm
+

lipli
>

111

co

*r

CO

CO
to

c-

C0
CM

CM

to

00
CD
CO

CO

CO
CO

CM

to

CM
CS

o
CM

Hill
llilll

P3

H
O^

HS
JH
$

HO
ZO

CO

CO

o
d

CO

o
d

CO

CO

o
d

CO

CO

o
d

CO

HH
Q<
a

E3

$
g
^

CU

Cu

cu

Z
O
HH

H
Z

El

s s

<

H
P

Bu

2
O

iSHiii

si

iglplll

<
aa

a
+
c

illplil
H

6-193

gQ
+
CO
Q

U
a.
+
CQ
03

<

Ti-6Ai-4V
:*:::*::;::::::;:::;:;:;:;:
>:::^:::>:|::::::::::;:::::
||g||||

CM

o
o
I:::***!

:.

'

o
o

;*a;

/-.

.5

02

U3
CO

lO
CO

CM

*T

CO

v*,

Be

*M

:'

i&;iw;&;
i:

H
Z

50

CO

CM

lO

o
ei

CQ
CO

_,

<1
*

o
Q
W
Q

ti

t^
C.
H

o
N

cy-

i-3

Z
O

"H

lpi|iii

~*

"*

CO

CO

lO

!;

^^
lI

ed

F-i

I|I11II

cd
W

S
op
J

<

Z
H
HH

llll

63

0.

A<

IB

Z
O
HH
H

111

SI?:?;

^Z:|:- ::
;
lpllil
:
' i* >

si

1
6-194

Ti-6A1-4V

:
*HtO

o
O
SSS

<-*>.

.a

till!

03
V

:^;iS^;;;;;;:;S;

o
i-t

'&0&&W
>

as

Mm

*.

JO

c<

''-&**

g* N_>

CO

to

gg
oy

GO

Ed

Sa.

op
s5

-t 3

ffl

9H
Q<

W
ffl

6-195

T1-6A1-4V

CM

?so::
: >-<
o

00

*o

io

5
02

CO
*1

mmtSm
00

CD
O

o*

llpl:

SSSSSSSSSSS

O
mmmm

fiilii mumm 11
y lllllll
!

<3 lil

id

Z
Z

Cti

*,-,
H

c>

"^

fa

CO
CO*
:; :'.':-

^>-:r^

3^
SB
op
gfe

At

OH

s-ii;

fill

O
14
H
<
H

Z
H
t4

ft-:>>:'ft

litifillf
iiUlillil
mmmkm%

<

SplllI ill

6-196

Ti-6A1-4V

CM

a
SSOK

-<

to

<
fe

C>

Ja

*H

co

Z
H
H

Z
ii
CO
CO

CD

O
PS

fe
o3

LEVELS
TEMPEI

s
3

illlil!

tf 9
Htf

CO p

CO

Q
WO

ov~
&3 N

00

zo
E
HH

Q<
H>

o
d

iVV

< 1*

Bg

g^

S
R

OK

o
h-1
H

1o

iipi
lipiiii

rs
H

hH
tf

p^B
s-i ^

iifiifili

l&illi

oH
03
Q

+
CO
Q

Ob

6-197

Ti-6A1-4V

ssiej

<3

::::
-<

o
o
JO

/rs

.5

H
Z

CO

oi

SStffi:

eg

J2

o
CO

t-

iil&*

iiiii

pII

55
0

en

<y~
sill

e4

msgmmm

~*

-*

00

CO

a.

a.

co

11

CD

^:-;'".'

w
N

spill
B
lgIIi
oo

P<

:|ij$

en

flli

D
O

Z
O
M
H
<
H
Z
W
M
tf

4SSS

H
Z

ill;?
:;:;:-:::-:::-:
jilll

5s
liliii
S"1 i#<
RS

&

:::

: : ::;*

iBiliii
:|:l*O c-,

E->

6-198

I
o
^t

o
c
o

/~.

t
t-

.S

3
?;
H

::>:::::.+.*:*::*

liiii

3
p lull
lull

00

(N

tr

a
z

o
o

PS
C"J

IC

o*^
rxt4

c*

CO

es

gs

DJ

o
fc.

PS

u.

a
o

t.

^ :-V.-

OG

es
n

z
o

<
H

ll
8g
8

D
H
J

o
o

o
o

e
2.

5
X

w
O
O
U
c

b.
o
o
o

b.
o
o
o

X
Ei.
o

b.
o

US
M3

6-199

T1-6A1-4V;

CM

SSD*
SKefe
o

.33

c
0 lilsi

be

sgSSKS8!

y"*

%
***

3
o

lilt*

1
III
B

uz

*d

Z
O

c4

ff-.
fil N

10

O
Z

ei
CO
iH
CD

-a: :;'..*

RDUC
FORM

IplIIII
ti

1o
fc.

*.

H
<
H
1-4

- v: Z

3o
o

i^W

O
O
c

lifgllll
llllpfllll
W

1
**$:
ssss?

Hl

&
5
p
8o

6.
o

"*

s
o

6-200

TL-6A1-4V

d
*SOH

*-*

IHI 5
SKO?
S;S*Q?

'T>

ft

III|SI

inn
ww&msi

H9

CO

:>W::iW(;ftW:::

o
es wsmmm

H
Z

CM

IO

CO

~H

o>

GO

us

t-

0
CM
CO

CO

14

CM
GO

CD
CD

OJ

IN
CO

&

fe.

Z
O

tf

w
CO

O1^

o
CO

* "^

CO

kO

CO

tO

CO

CO

id
CN

CO

CM

CM

CO

US

CD
CO

*-^.'

o
d

RODUC
FORM

...&*

Pk

CO

z
H

s0

a
a
E
5
w

a.
to
Z
3

Si

z
o

::

CD

CM

>H

Silil
pilii

^H

Of

&

>

ft.
a
iC 00

>

CD

1
Bi
X

111

a
E
5
u
a.
2
D

CO

O EH

fc.

Er,
o

b.

6-201

Ti-61-4V

o
o
was

IS

CO
l

es
ei

CM

CM

co

co
CM

CM

'.:

CO
CO

t-

00
c

ill

CO

CO
eg

lll

c4

O
CO

CO

c
W

.v.,- '; ;\

co
d

Sa

D
H
ta

Cd

CD

U
ta
c
to
2
D

H
Z
55

52 ISS

OK

<

es

E
fc.

CO

o.

OH

6-202

O
to

z
D

T1-6A1-4V

I
M
^*

rfgi?

3ps4

g3
X
Of
U
f

z
o

s
cd
CO

id
ii*
|||

fc o

BIG

eg*

I
8

S3

S3

to to

CO to

88

88

u. u.

6-203

"6

%i

%l

r<

ii

fa 8

- o

T1-6A1-4V

I
5>
ifi

*l%

iii<

H
Z
O

of

Of
K

3
Ed
a

J
o

i dps

cd
CO

ii*
o

9PS

a. o

eg-

Si

ij

E"

E3

fi

s!

si

BS

E-

E-

BJ

Bi

E-

EBj

E"
PS

gs
5

'.s

of

85

Of

O
EU

b. <
fa

~ o

si
S

6-204

K fc.

1
6. "

Of <

fa.

B.

it

III

Ti-6A1-4V

I
5>

^
^5L2

i E D

o
to

z
SIB

Sen

CO

|i*

ft. o

$2

I
o
u

* o 3
w "9 e z

ai
SKP>?8P

6-205

Ti-6A1-4V

g 2

2 g

I
5>
t/S
*&

Q
H
P
Z
O

so*

3
z
S
09

E-

H
Q

oa
a.
OB

CD

i*
9*3

fe o
E-

E-

'S

I*
a
o

6-206

T1-6A1-4V

OS

l
is
rf!

fan

Q
H

Pi

P
Z

tf

z
o

z
g
S
H
a

CO
CP

i>
3|

a. o
I"

I
ea
e

8
a.

c
0

5
'S

Z
o

E
s
a

z
o

o <

6-207

o
u

Ti-6A1-4V

as

I
is
X

'a?
00

a
T

Szzl

M
2

s
S

CO
1-4

0.
00

i*

9p5

g
&o

ob

ob

frei

fr
s

eu

as

ss

-u

<

6-208

SS
<

Ti-6A1-4V

I
5>
^j

tf

rfg"!
GO

3 4

111
2

a
CO
CO

**

9es
Mtf

P. o

feie

Oil

E-

si

Si

r
a

a.

"6

I
Q

a
2

BS

85

S3

SS

a
u

W S

<

o
z

6-209

Ti-6Al-4Vi

I
5>

rf?
s

i^SU

P
D
H

55

us
z
8oo

S-i

E-

EU

EO

H
ft.

id

i*
e

9g?

pi

8g

6
g
oEb

6-210

Ti-6A14V

si

I
is
rfs

tf

rfjH

Q
H

P
ii

BE-

6S
*

z
o
S

i
B-
Sen

so

go

CD

!i*

in
is
P. o

E"

feic

E-

SB

a!

20aa S

H W Q
5 H

ill
05 S

e 1
Q O
K 2
a H

P3

a
Oases
wo*

B - ;> <
fc

E-

'S

Ob

ggi

Q P3
K
O S
Z
^

B < "* i
aas

M (0S

6-211

2dl

(BBlg-

CD 03 C *+

as

I
2>

tii

*i%
P,2
3^
Q

P
Z
I4
H

E
U

EU

EH

B?.

cd
CP

i*
PQ

gSl
H g
O

&

cd

E-

6(6

E-

|3~
B

'S
<2

2
Q

O
U

B
B O
En<
OS
5
a H a c 5 ;

S3
S '
ca

2
O _ Jl
E" a C Z "*

SBSoS
3BHs

oga
"
o -

ps5
5 81111
IP
a<
B? 32 D

_pa **
w 3
< * d
s
10(0

IS

6-212

T1-6AI-4V

I
Is
j

*l9
U9

-IT
Q
H

P
Z
H
Z

o
o

M
2

EU

ES

i*

gu
&

03

OS

a*
o

0.

Q Q J5 O

z
o

aligns
zS25S5

<aa

ao
H

A3 S < BJ j g

SHaS32

B3 03 25

SIQOSOSPS

03 W S *

Sn2

<

i
K <

6-213

-R-61-4V

OS

I
5>

rf|

tfan
00

'I
Q
P

S3

Six

H
Z
O
O

as
o

IB

M
Q

E8
11

i*

N
9es
H

sag

Sgal

5 P e
pa g a S

S U -4 ^

ss aa ^
2 z
fc.

a -g

o 5 6. p

-g

6-214

Ti-6Ai-4V

SS

I
is
M

?!

rfsu
3^2

p
P

BE6S

o
CO

CB

id

CO

I i*

gli
H

H BS

els

BS

BS

Oil

Ei

EBS

PS

BS

a
S

b b Z j

88B(
z
o *-.- *^i W p b b

!S

6. &> z S

ggug
S " ""

? o gs
BgS;

b b Z S
5 e * g t.

288SE

b H U b b

01 b H p b b

2 " ""

=>

5g

b b Z S

so _

gl

6-215

*5!

Ex, b Z fi

b b Z fi

2"

>

m PBz
3Bi"5 =
b B p b b
&gbg g
Q Z BS S 5

B55g

01

*2Sz

b H U b b

b b Z fi

*88gg
5 t- ^ E f
2 "" ""

b B p b b

sisg

T1-6A1-4V!

I
5>
is
tf

^i
T
el,
zl

D
Z

M
z
2
x

ooz

id

E8
CO

ii*
SP?

eg8-

Pi

Si

g3
B

S
z
o

o " <-" " ,


S i OS;

ppPig!
6< B P fe I
fegSg;

&$S3

ip* ^ 9s <z&i

s^
22
s <
z &<

05

S Ei"

6-216

81

Si

T1-6A1-4V

as

S3

su
z

is
bfe

sPi

t^SU

5 1

P
H
P

Ml

o
o
CO

81-3

*i<

Of
H

Sa

ft.

Id

OD

CO

'i*

9*s

H PS

E-i

gg

E-i

P.

f-l

E-

EBS

Ei

g
a!

ai

Si

Ia
s

sa

2
w

z
o

a
2
o

<z

<
d

6-217

K-6A1-4V

I
is
kfS

rfg

00

D
Z
H
Z
O

ill"
W
2

CO
M

CO

id
go

to
ii*

gig

s
8d

S:

is

t"

Sic

J
fi

Si

Pi

Is
-8

58
is

fig

E
'S
u

H S
^2
t- 3

5a

'S

2&>

a
a

is

*= BS
X
SE

< 6.

^8

*8

6-218

IB

IS
-58

3
< 6.

^8

uP

en S

B9

N
11
^
fe!

53

SSJ

Ti-6AI-4V

I
5>

is
rf!

s
s

rfgi?

III

Z
H
Z
O
O

s
s

M
as
o

H
Q

5?
CD
i-i

|i*

9et
>

g
as

11188
^ ' 2 SS

6-219

T*6A1-4V
3
s

s
8

I
is
tf

rfan
W
w
p

si

ii

er
u

SB
O

6->

H
Q

cd

i*
PQ

gig
&o

Be6

si

|3
s

a. & ri a

I
cu

a5ooB
3 5 S v ^
c ij *" 5

2 < y S fe
gaSg
|

gi
6-220

Ti-6Al-4Vi

as

ES

I
5>

rfS

^I'l
3??

Si-

Q
H

P
M

SO

H
Q

2
eo

i-H
CO

li*

gig
&o

BJ

1
a
o

., fc & rf S

H S O X

a
2OB
asses
S "^ P & fe

SMS

6-221

ll-SAMY

I
is
&

uf2

rfStf

P
Z

isU

z
o

2
0

5:

S dB

B8

i>

Ss

I!

" o
>

5 B

?1

ilisi
N 2 O "H

ilBii

6-222

EU

iTi-6Al-4V!

OS

I
3>
is

rfS

rfgll

a
Q

ill**

as
g

E->

i "3B
CO
CO

i*

gig

eg*

1*
isg

I
p.

S o 9 O ffi

asSoE
< P5S

SuSSs

6-223

^61-4V

s
3>
is

rfS

'88
0< ^

8si*5

zg

tu
M
Q

Irin
CD

i*

9es

CO

&

fei -

S3
=3

?1

HQ
^ fe
N
S S
QX

2 " SSS2

6-224

CO

-6A1-4V

I
is
rfs

Q
H
Q

ug

!!<

2
a
m

CO
CO

i*

gig
H K
& O

J is

a!)

5K =

03 fx, & 5? BS

|llf

i 1111 s
we K

sa

fs

S o 2 O g
S3 5 g o IS

J52uS

g gSS

g||ll

2
or

ft*

6-225

T1-6A1-4V

8
S

I
2>

*:

rfl
5>

4
i
Ss
CO
F-l
CD

5:

si
59

in
2

&
OB

12*
9P?

a, o

Jl

Jl

Jt

Jl

6-

8-
3
O

a.

<
BS
B

fa
s

BS

x
fa
S

6-226

\-Ti-6A14V

I
is
MTS

rfl
2>

a
a

&5

CO

]7i
6g

&
Q

Hi

d
s
S
z

CO

Hit)

2*

OS

a
z

Sei

sei
M

In

te

E-

E-

EO

BSlC
fc

ei

^ e

E->

si

E-

E"
K

ft.

z
o

B
H

33

HI

ii

z
z

6-227

I
2>

1B
b?t

*1
5>

J\

A
?

o
u

fc

CO

65"

S="
go
see

o
to
o

S*

E-

P5

P |2 ^

si

EBS

6-228

T1-6A1-4V

I
2>

u?!

rfl

is
w

A
A

rf

2ii

! C *
! S

ii*

&o

J
E-

E-

EK

80.

6-229

I Ti-6AI-4V I
Condition/Ht:
Form:
Specimen Type:
Orientation:
Frequency: 30 Hz
Environment: LAB AIR; RT

Yield Strength:
Ult. Strength:
Specimen Thk: 0.081 in.
Specimen Width: 2.5 in.
Ref: PW003
(1 of 1)

AK (MPaVin)
4

10

' I 'I'l'l

AK (MPaVin)
1

40
100
-ii i i I nil

10

b I ' I 'I'l'l

40

100

' I 'I'l'l

10

Stress Ratio: 0.1

10

10

10
-i

10

10

-3

10

10

fci o"

10

o
_
frltf"4

a>

-2-

-2 '

-3 I

10

,-s

10

10

10

10

"a

10

10

10
10

10

-6

10

10
.-8

10

'

I I I I Hi
4
10

-8

10

I M III

40

'

da/dN (10_6in/cycle)

AK (KsiVin)

0.125
0.242
0.328

6.09 (min)
7.
8.
9.
10.
12.31 (max)

0.601
1.33
2.80

Life Prediction Ratio Summary


i

0.

10

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

I I I llll
40
100

I I I I II

100

AK (KsiVin)

RMS %
Error
10.38

_
10

.5

.8

RMS %
Error

1.25

Life Prediction Ratio Summary


r

.5 .8

2.

Figure 6.16.3.1.1
6-230

1.25

i-'

2.

This page intentionally left blank

6-231

\ Ti-6AI-4V h
Condition/Ht:
Form:
Specimen Type: CT
Orientation: C-R
Frequency: 20 Hz
Environment: LAB AIR; RT

Yield Strength:
Ult. Strength:
Specimen Thk: 0.28 - 0.299 in.
Specimen Width: 2.5 in.
Ref: PW003
(1 of 4)

AK (MPaVin)
4

10

40

(2 of 4)

AK (MPaVin)
4

100

10

40

100

i I i I HU

= I ' I 'IT

i I M 'Ml

Stress Ratio: 0.3


10

-3

10

o 10

10
o

10

10

.-8

10
4

10

40

100

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error
12.87

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

40

100

da/dN (10-6in/cycle)

AK (KsiVin)

0.198
0.403
0.898
1.66
4.48
8.73
16.3
21.2

7.27 (min)
8.
9.
10.
13.
16.
20.
21.70 (max)

1.31
2.86
5.86
10.4
17.8
31.2
58.9
121.
142.

11.07 (min)
13.
16.
20.
25.
30.
35.
4-0.
41.03 (max)

10

AK (KsiVin)

2.

RMS %
Error
17.18

Figure 6.16.3.1.2
6-232

Life Prediction Ratio Summary


.5

,8

1.25

-I Ti-6AI-4V
Condition/Ht:
Form:
Specimen Type: CT
Orientation: CR
Frequency: 20 Hz
Environment: LAB AIR; RT

Yield Strength:
Ult. Strength:
Specimen Thk: 0.28 - 0.299 in.
Specimen Width: 2.5 in.
Ref: PW003
(3 of 4)

AK (MPaVin)
4

10

40

(4 of 4)

AK (MPaVin)
1

100

b I

10

' I 'I'l'l

40

100
1

' I 'I' "

10

Stress Ratio: 0.5


-2

10

:
10
o
o 10

2
io" ^

10

:
10

. :
-

_x"0
10

10

10

nffi

10
10
10

~ I , I, I,I,
4

I , I , E,l.

10

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error
28.66

0.

.5

.8

100

1.25

3.07 (min)
3.5
4.
5.

0.0347
0.0467
0.0702
0.154

6.
7.
8.

0.295
0.545
1.04
1.82

8.80 (max)

Life Prediction Ratio Summary


i

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.102
0.161
0.333
0.664
1.16
1.82
5.28
12.3
18.2

5.18 (min)
6.
7.
8.
9.
10.
13.
16.
18.26 (max)

10

AK (KsiVin)

AK (KsiVin)

i-'

2.

RMS %
Error
12.39

Life Prediction Ratio Summary


i

0.

Figure 6.16.3.1.2 (Concluded)


6-233

.5

.8

1.25

2.

\ Ti-6AI-4V
Condition/Ht:
Form:
Specimen Type: CCP (max load specified)
Orientation: C-R
Frequency: 0.2 Hz
Environment: LAB AIR; RT
(1 of 2)

AK (MPaVin)
1

10

- i i M'l'i

Yield Strength:
Ult. Strength:
Specimen Thk: 0.299 - 0.301 in.
Specimen Width: 2.5 in.
Ref: PW003

40
100
Ii I i I'l'l

Stress Ratio: -1.0

(2 of 2)

AK (MPaVin)
1

- I

m
10

10

' I 'I'l'l

40

100

' I 'I'l'l

Stress Ratio: -0.5

10

10

10

-2

-1

10

10

-3

10

10

jo

-no"2

JD

_0>

o^10-

10

6^10-4

10

XI

10

o
x>

10

10

10

10
10

10

10

10
'

I I I III

I Ml

10

40

'

10

I III!

100

Life Prediction Ratio Summary


0.

.5

.8

1.25

100

0.314
0.783
1.21
3.67
11.1
12.2

8.19 (min)
9.
10.
13.
16.
16.57 (max)

0.783
0.847
1.14
3.96
12.5
19.7

8.55 (min)
9.
10.
13.
16.
17.54 (max)

I I I III

40

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
6.59

10

10

10

10

RMS %
Error
15.36

Figure 6.16.3.1.3
6-234

Life Prediction Ratio Summary


i

0.

.5

.8

1-

1.25

\ TI-6AI-4V r
Condition/Ht:
Form:
Specimen Type: CCP (max load specified)
Orientation: C-R
Frequency: 0.2 Hz
Environment: LAB AIR;300F

10

40

Yield Strength:
Ult. Strength:
Specimen Thk: 0.297 - 0.302 in.
Specimen Width: 2.5 in.
Ref: PW003

(1 of 2)

AK (MPaVin)

(2 of 2)

AK (MPaVin)
4

100

1I I 11 M'l

- i ' i M'l'ir

10
I HM|

40
100
1I | I | mi

10

Stress Ratio: -1.0


10

10
-3

10

0)

o 10

10

10

10
T3

10
10
10
10

10

LI

I I I 11II

I I I I III

10

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

RMS X
Error
22.59

i-i

.5

.8

100

1.25

0.242
0.473
0.912
3.21
5.81
16.4

8.12 (min)
9.
10.
13.
16.
18.48 (max)

Life Prediction Ratio Summary


0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.752
1.03
1.32
3.51
9.52
14.3

8.26 (min)
9.
10.
13.
16.
18.42 (max)

10

AK (KsiVin)

AK (KsiVin)

i-'

2.

RMS %
Error
27.78

Figure 6.16.3.1.4
6-235

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

-\ Ti-6AI-4V I

Condition/Ht: 1550F 4HRS FC 1000F 4HRS ARGON COOLED


Form: Forging
Yield Strength: 140.9 ksi
Specimen Type: WOL
Ult. Strength: 150.1 ksi
Orientation: R-C
Specimen Thk: 0.8 in.
Stress Ratio: 0.1
Specimen Width: 2.55 in.
Frequency: 10 Hz
Ref: UM001
(1 of 1)

AK (MPaVin)
4

10

40

-Ml 'I'l'l

100

I ' I 'I'l'l

Environment: Argon; R.T.

AK (MPaVin)
1

10

40

' I 'I'l'lI

100

' I 'I'l'l

~ 10

10

-2

10

10

10

10

10

10

io"
o
\

10

-a
10 \
D

^10"
c

2 10"5

-a

_fi r10

_aj

o
\

u
_
frio-4

-3 |

10

E
a

10
~

10

10

w*

10

10
10

10

10

10
10

"

I , I, I,I,
4

I , I,I,I,

10

40

10

100

da/dN (10_<in/cycle)

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.241
0.805
1.96
4.31
8.49
17.3
46.0
166.
390.

10.00 (min)
13.
16.
20.
25.
30.
35.
40.
44.83 (max)

RMS %
Error
30.58

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

inn

' i i iHI
4
10

Life Prediction Ratio Summary


i

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary

i-'

0.

2.

Figure 6.16.3.1.5
6-236

.5

.8

1.25

J
I

Condition/Ht: 1750F 4HRS ARGON COOLED


Form: Forging
Specimen Type: WOL
Orientation: R-C
Stress Ratio: 0.1
Frequency: 10 Hz
(1

AK (MPaVin)
1

10

40

of 1)

AK (MPaVin)
1

10

10

= I ' I ' I'l'l

40

100

' I 'ITI

-1

-1

-i

10

10

la"3

io"2

u 10
\

2M0"S

MT

10

\
D
~V

10

10"2

ID"2

ID"3

I _

Yield Strength: 135.7 ksi


Ult. Strength: 144.9 ksi
Specimen Thk: 0.8 in.
Specimen Width: 2.55 in.
Ref: UM001

100

- Environment: Argon; R.T.

-r:
PAi
A\
I I DMI tV

-z.

Z10"5

>

\
o
"

-6

10

10
-

io-7

IQ"7

-6

-6

10

10

~l,l ,1,1,
4

I , I , l,l,

10

40

_ 1 , 1,1,1,

10"8
1

100

da/dN (10"6in/cycle)

10.46 (min)
13.
16.
20.
25.
30.
35.
40.
43.64 (max)

RMS %
Error
43.72

10

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.190
0.613
1.70
4.38
9.53
19.8
50.4
176.
553.

Life Prediction Ratio Summary


0.

I , I,I,I,

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

>

-5

-5

10

10"8

10

-6
10

.5

.8

1.25

2.

RMS %
Error

Life Prediction Ratio Summary


0.

Figure 6.16.3.1.6
6-237

.5

.8

1.25

2.

^ Ti-6AI-4V r
Condition/Ht: 1750F. 4HRS ARGON COOLED
Form: Forging
Specimen Type: WOL
Orientation: C-R
Stress Ratio: 0.1
Frequency: 10 Hz
(1 of 1)

AK (MPaVin)
4

_ |

10

i | 11' t M

40

Yield Strength: 135.7 ksi


Ult. Strength: 144.9 ksi
Specimen Thk: 0.8 in.
Specimen Width: 2.55 in.
Ref: UM001

AK (MPaVin)
1

100

' I M'l'l

Environment: Argon; R;T;

- I

40

100

' I M'l'l

10
10

10

10

10

-5>
o

3M O"
c

,0-1

6^10-'

10~

-A.-0

10

I
z.

Z 10

10

<D

2
10~
o
\

m~ ^
u

-o

10

10

*~"

10

10
10

III 1

10

10

' I M'l'l

10

10

10

10

1 , 1,1,1,

10
4

10

40

-8

10

100

da/dN (10"6in/cycle)

AK (KsiVin)
16.
20.
25.
30.
35.
40.
40.42 (max)

Life Prediction Ratio Summary


0.

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.294
0.615
1.84
5.00
11.1
26.1
63.1
296.
360.

10.71 (min)

13.

RMS %
Error
21.49

10

AK (KsiVin)

AK (KsiVin)

.5

.8

RMS %
Error

Life Prediction Ratio Summary


0.

1.25

Figure 6.16.3.1.7
6-238

.5

.8

1.25

-I Ti-6AI-4V h
Condition/Ht: 1775F 1HR WQ 1675F 1HR WQ 1000F 4HR AC
Form: 0.5 in. Disk
Yield Strength: 120 ksi
Specimen Type: CCP (max load specified)
Ult. Strength: 130 ksi
Orientation: C-R
Specimen Thk: 0.12 in.
Stress Ratio: 0.05
Specimen Width: 1.98 in.
Frequency: 0.3 - 10 Hz
Ref: GE003
(1 of 2)

AK (MPaVin)
4
F=Ii

10

40

100

-ii i i I ill

FT

I i I'M

Environment: Lab Air; R.T.

(2 of 2)

AK (MPaVin)
- I

4
10
' I 'I'l'l

40

100

1i l i 11111

Environment: Lab Air; 200T

10

10

10

10

10
10

10

-5>

io"2
o

10

Z 10

10

10

o
-o

10

10

10
-7

10

10

10

LI

i in
4
10

10

1.1.1
40

-8

'

10

100

RMS %
Error
3.86

.5

.8

100

1.25

50.8

30.79 (min)
35.
40.
50.

38.7
57.9
80.3
162.
286.
590.
1635.
1718.

94.7
168.

357.
737.

60.
70.

1832.
2860.

74.44 (max)

Life Prediction Ratio Summary


a
0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (lO^in/cycle)

30.47 (min)
35.
40.
50.
60.
70.
80.
80.58 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , I,I,I

I I INI

RMS %
Error
5.23

Figure 6.16.3.1.8
6-239

Life Prediction Ratio Summary


-r-

0.

.5

,
.8

,
1.25

,
2.

TJ-6AI-4V I
Condition/Ht: 1775F 1HR WQ 1675F 1HR WQ 1000F-1200F 2-8HR AC
Form: 0.94 - 1.15 in. Disk
Yield Strength: 145 - 150 ksi
Specimen Type: KB Bar
Ult. Strength:
Orientation: C-R
Specimen Thk: 0.251 - 0.253 in.
Frequency: 0.3 Hz
Specimen Width: 0.995 - 1.002 in
Environment: LAB AIR;600F
Ref: GE007
(1 of 3)

AK (MPaVin)
4

10

40

100

- I

- I i I M'l'l
I ' I Tl'l
Stress Ratio: 0.03

10

i I M'l'l

40

100
a

' I M'l'l

Stress Ratio: 0.25

10

-2

10

10

-1

10

:
10

10

io"2

0)
o

i o"
c

-2 '

h-

Q>

10

10

10

-Jio
>

Z 10

10

o
~

(2 of 3)

AK (MPaVin)

Jio
>

-6

-a

10

10

-5

"""

10

-r: 10

10

10

-=

10
.-8

10

" 1 - I.I.I.
4

1 , 1,1,1,

10

40

10

" I , I.I.I.
4

100

RMS %
Error
22.00

40

100

da/dN (10"6in/cycle)
1.96
2.06
3.61
7.04

9.28 (min)
10.
13.
16.
20.
25.
30.
30.82 (max)

0.600
0.864
1.24
3.17
6.31
11.5
19.7
32.2

13.7
21.5

30.1
31.9

51.2
68.1
65.3

Life Prediction Ratio Summary


0.

10

AK (KsiVin)

da/dN (10"6in/cycle)

8.01 (min)
9.
10.
13.
16.
20.
25.
30.
35.
40.
42.82 (max)

I , I . LI.

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

.5

.8

1.25

RMS %
Error
12.30

Figure 6.16.3.1.9
6-240

Life Prediction Ratio Summary


i

.5

.8

1.25

U-6AI-4V h

Condition/Ht: 1775F 1HR WQ 1675F 1HR WQ 1000F-1200F 2-8HR AC


Form: 0.94 - 1.15 in. Disk
Yield Strength: 145 - 150 ksi
Specimen Type: KB Bar
Ult. Strength:
Orientation: C-R
Specimen Thk: 0.251 - 0.253 in.
Frequency: 0.3 Hz
Specimen Width: 0.995 - 1.002 in
Environment: LAB AIR;600F
Ref: GE007
(3 of 3)

AK (MPaVin)
1

10

40

- i i 'I'i'i
r
Stress Ratio: 0.54

"II

AK (MPaVin)
4

100

40

100

I ' I 'I'I'I

10

10

-2

10

10

10

10

10

10

io"
2

_Q5
O

_0

o
G^O-4

o10"
c
_
10

10

- I ' I'l'l'l

I I I MM

-3 I

10

-5

10"

10"

~ 10-6|-

X3

(~
m '\
u
D

10

"

10
-7

10

10

10

10

10
'

10
4

10

10

I I I III

40

100

100

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary

0.

40

1.96
1.96
2.12
4.38
8.94
13.6

8.94 (min)
9.
10.
13.
16.
19.48 (max)

RMS %
Error

10

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

I . 1,1,1,

- I , l,l,l,

AK (KsiVin)

14.60

3E

10

.5

.8

RMS %
Error

Life Prediction Ratio Summary


,

0.

1.25

Figure 6.16.3.1.9 (Concluded)


6-241

.5

1i

.8

1.25

2.

\ Ti-6AI-4V I

"

Condition/Ht: 1775F 1HR WQ 1675F 1HR WQ 1000F-1200F 2-8HR AC


Form: 0.94 in. Disk
Yield Strength: 150 ksi
Specimen Type: KB Bar
Ult. Strength:
Orientation: C-R
Specimen Thk: 0.252 in.
Frequency: 0.3 Hz
Specimen Width: 0.991 - 0.999 in
Environment: LAB AIR;300F
Ref: GE007
(1 of 3)

AK (MPaVin)
4

10

40

100

- I I ll>l>l
I ' I 'l'l'l
Stress Ratio: 0.03

10

100

-1

Stress Ratio: 0.25

10

io"2^
o

10

-3

10

10

_0)

io"2
o
\

o 10
\
c

40

I ' I 'l'l'l

10

10

= I ' I 'I'l'l

10

-3

(2 of 3)

AK (MPaVin)

ZIG"5
"D
p

o
6^10-4

-3 |

-3 |

10

10

-= 10

Z 10

Jio
>

:
"o _K r10

-o

-o

_*
10

10

10

10

10

10

10

"

I , LI,I,

I , l,l,l,

40

10

10

" 1 , 1,1,1,
4

100

da/dN (10"6in/cycle)

RMS %
Error
14.98

40

100

da/dN (10"6in/cycle)
1.46
3.46
6.88
11.9
20.9
39.8
60.4

10.90 (min)

13.
16.
20.
25.
30.

4.92
9.75
19.7
34.6
53.3
76.6

32.83 (max)

82.6

Life Prediction Ratio Summary


r-

0.

10

AK (KsiVin)

0.644
0.709
2.40

9.83 (min)
10.
13.
16.
20.
25.
30.
35.
40.
41.12 (max)

1 , 1,1,1,

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

.8

1.25

RMS %
Error
22.63

Figure 6.16.3.1.10
6-242

Life Prediction Ratio Summary


i--

0.

.5

.8

1.25

2.

\ H-6AI-4V

Condition/Ht: 1775F 1HR WQ 1675F 1HR WQ 1000F-1200F 2-8HR AC


Form: 0.94 in. Disk
Yield Strength: 150 ksi
Specimen Type: KB Bar
Ult. Strength:
Orientation: C-R
Specimen Thk: 0.252 in.
Frequency: 0.3 Hz
Specimen Width: 0.991 - 0.999 in
Environment: LAB AIR;300F
Ref: GE007
(3 of 3)

AK (MPaVin)
1

- I

10

I 'I'l'l

40

AK (MPaVin)
4

100

' I M'l'l

Stress Ratio: 0.54

10

40
i

i 111

100

rr

iii

10

10
-2

10

10

10

10
10

10

-2

_Q5
U

O 10

TJ

3
10- E

10

10

10
10

o
6-10-4
_c
_

10

-5

10

o
10

10
10

10

10

10

1111 in

' i i mi

10

40

10

Life Prediction Ratio Summary


i

0.

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

3.45
5.10
8.22
11.5

11.42 (min)
13.
16.
18.98 (max)

6.81

10

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

I , Ml

i 111in
JiL
4

100

AK (KsiVin)

RMS %
Error

T3

10

10

ii

.5

.8

1.25

2.

RMS %
Error

-Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

Figure 6.16.3.1.10 (Concluded)


6-243

] Ti-6AI-4V I

Condition/Ht: 1775F 1HR WQ 1675F 1HR WQ 1000F-1200F 2-8HR AC


Form: 0.94 in. Disk
Yield Strength: 150 ksi
Specimen Type: KB Bar
Ult. Strength:
Orientation: C-R
Specimen Thk: 0.251 - 0.252 in.
Frequency: 0.3 Hz
Specimen Width: 0.996 - 1 in.
Environment: LAB AIR; RT
Ref: GE007
(1 of 3)

AK (MPaVin)
4

- I
-2

10

10
jD

o 10

Z 10

10

' I 'I'l'l

40

' I 'I'l'l

10

.-8

10

i]

z 10
XI

, I,I,I,
4

, I,I,I,

10

40

10
10
10

10

JA

10

100

RMS %
Error
27.22

Life Prediction Ratio Summary


0.

.5

.8

1.25

100

2.70
4.59
9.26
22.1
41.5
76.2

11.13 (min)
13.
16.
20.
25.
29.06 (max)

18.0
24.2

111iii

40

da/dN (10-6in/cycle)

AK (KsiVin)

0.744
0.822
3.27
6.67
11.5

10

AK (KsiVin)

da/dN (10"6in/cycle)

9.85 (min)
10.
13.
16.
20.
25.
28.66 (max)

AK (KsiVin)
AK (KsiVin)

iXJ

10

10

"

10

__
-5
10

1.0

o
o 10

- io"'\
o

10

10

*""*

Ir ' I 'I'l'l

10

100

10

-3
I
10

40

Stress Ratio: 0.25

_0J

2
10"

10

- i ' i 'i'i'i

"_L

-1
10

100

- Stress Ratio: 0.03

(2 of 3)

AK (MPaVin)

RMS %
Error
5.32

Figure 6.16.3.1.11
6-244

Life Prediction Ratio Summary


0.

.5

.8

1.25

1 T;

P.A I

AM

Condition/Ht: 1775F 1HR WC) 1675F 1HR WQ 1000F-1200F 2-8HR AC


Yield Strength: 150 ksi
Form: 0.94 in. Disk
Ult. Strength:
Specimen Type: KB Bar
Specimen
Thk: 0.251 - 0.252 in.
Orientation: CR
Specimen
Width: 0.996 - 1 in.
Frequency: 0.3 Hz
Ref: GE007
Environment: LAB AIR; RT

(3 of 3)

AK (MPaVin)
1

10

40

-I'M I'l'l

AK (MPaVin)
1

100

_i

I'M I'l'l

= I

10

' I ' I'l'l

40
I

100
-1

' I 'I'l'l

10

Stress Ratio: 0.54

IQ"2

ID"2

-1

10

10
ID"3

^^

_~

10"3

io"2

"a?

a;

^10"

o
\

o
o^10-4
\
c

C^*

"^s

**-*

2 10"5

ZIG"5

X!

10

^"^
-z.

\
o

\
O

10

-6

10

-5

-5

10

10

.
_

IQ'7

10

ID"

-6

10

1C)0

40

- 1 , 1,1,1,

m"8

I , I , l,l.

" I , I . I . I.

M?*

6
da/dN (10 " in/cycle)

10.48 (min)
13.
16.
19.06 (max)

RMS %
Error
13.84

3
6
12
16

.5

.8

100

27
41
1
6

RMS %
Error

1.25

40

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Rati 3 Summary


0.

I , I,I,I,

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

-6

10

10

Life Prediction Ratio Summary


0.

2.

Figure 6.16.3.1.11 (Concluded)


6-245

.5

.8

1.25

2.

^ Ti-6AI-4V
Condition/Ht: 1775F 1HR WQ 1675F 1HR WQ 1000F-1200F 2-8HR AC
Form: 0.94 in. Disk
Yield Strength: 150 ksi
Specimen Type: KB Bar
Ult. Strength:
Orientation: C-R
Specimen Thk: 0.251 - 0.252 in.
Frequency: 0.5 Hz
Specimen Width: 0.989 - 0.997 in
Environment: LAB AIR; RT
Ref: GE007
(1 of 2)

AK (MPaVin)
4

_~l

10

. I lITl

40

100

I I ITI

Stress Ratio: 0.03

10
-3

10
_qj

e
.-6

10

10

ZIG"5

-L

.-8

100

' I M'l'l

10

_2
10"2

10

-5

10

-T= 10

i I i I ili
4

1 ,1,1,1,

10

40

100

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

100

3.43
5.09
9.55
17.7
35.2
65.8
73.7

10.87 (min)
13.
16.
20.
25.
30.
30.68 (max)

5.90
9.93
18.3
32.2
57.6
107.
186.

16.74 (min)
20.
25.
30.
35.
40.
44.18 (max)

40

da/dN (10-6in/cycle)

AK (KsiVin)

da/dN (10-6in/cycle)

AK (KsiVin)

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
8.13

40

10

10

' I 'I'l'l

-3 |

ui

b I

10

(2 of 2)

AK (MPaVin)

RMS %
Error
4.71

Figure 6.16.3.1.12
6-246

Life Prediction Ratio Summary


!-

.5

.8

1.25

2.

TI-6AI-4V r
Condition/Ht: 1950F 4HRS WQ
Form: Forging
Specimen Type: WOL
Orientation: R-C
Stress Ratio: 0.1
Frequency: 10 Hz

1000F 4HRS ARGON COOLED


Yield Strength: 136.4 ksi
Ult. Strength: 147.8 ksi
Specimen Thk: 0.8 in.
Specimen Width: 2.55 in.
Ref: UM001
(1 Of 1)

AK (MPaVin)
1

- I

10

40
-I

' I M'l'l

AK (MPaVin)
1

100

i- I

II Mill

10

' I'l'l'l

40

100

' I Tl'l

10

Environment: Argon; R.T

-4

10

-2

10

10
10
o

o
o 10
_c
l_
D

-o

-5

10

.A.-0

10

_fi
10

10
-7

10

10
10
4

10

40

'

100

da/dN (10"6in/cycle)

10.04 (min)
13.
16.
20.
25.
30.
35.
40.
50.
50.06 (max)

RMS %
Error
61.91

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.187
0.492
1.12
2.52
5.06
10.7
26.8
68.3
148.
147.

Life Prediction Ratio Summary

RMS %
Error

-r-

0.

10

I I I I II

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'

''"I

.5

.8

1.25

2.

Figure 6.16.3.1.13
6-247

Life Prediction Ratio Summary


i

.5

.8

1.25

i--

2.

-\ T1-6AI-4V r
Condition/Ht: 1950F 4HRS WQ
Form: Forging
Specimen Type: WOL
Orientation: C-R
Stress Ratio: 0.1
Frequency: 10 Hz

(1 of 1)

AK (MPaVin)
4

10

1000F 4HRS ARGON COOLED


^eld Strength: 136.4 ksi
Ult. Strength: 147.8 ksi
Specimen Thk: 0.8 in.
Specimen Width: 2.55 in.
Ref: UM001
AK (MPaVin)
1

40
100
i I i H|i|

- |

10

40

'I M'l'l

100

' I 'I'l'l

10

10
10
10

d)

10~

o
o 10

10"

'1

^-^

-5

10

d T7
4

\
U
-u

10
10
-7

10

10

10,-e
4

10

40

100

AK (KsiVin)

100

0.196
0.410
1.28
3.63
8.51
17.9
67.7
84.8

Life Prediction Ratio Summary

RMS %
Error

.8

1.25

Life Prediction Ratio Summary


i

i-'

0.

40

da/dN (10-6in/cycle)

AK (KsiVin)

da/dN (I0_6in/cycle)

11.18 (min)
13.
16.
20.
25.
30.
35.
35.49 (max)

RMS %
Error
39.35

10

AK (KsiVin)

AK (KsiVin)

0.

2.

Figure 6.16.3.1.14
6-248

.5

.8

1.25

2.

This page intentionally left blank

6-249

^ TI-6AI-4V I
Condition/Ht: ALPHA-BETA FORGE-ANNEALED
Form: Forging
Specimen Type: CT
Orientation: LT
Stress Ratio: 0.1
Frequency: 30 Hz
(1 of 3)

AK (MPaVin)
4

10

40

' I 'I'l'lI

Yield Strength: 50 - 100 ksi


Ult. Strength:
Specimen Thk: 0.25 - 0.252 in.
Specimen Width: 1.993 - 2.01 in.
Ref: SA001

100

' I'l'l'l

Environment: Lab Air; R.T.;


Yield Strength: 50 Ksi

1
-

(2 of 3)

AK (MPaVin)
4

10

40

' I 'I'l'l

100

' I 'I'l'l

10

Environment: Lab Air; R.T.;


_ Yield Strength: 80 Ksi

10

-2

10

10

10

10
10

10*
_Q)

o
_
frio-4

o
\

u
fci o-+
c
_

XI

-3 |

10

-5

io"2

10

"O

10

x>

T3

_E

10

10

-s

_-

10

10

10

-B

-5

-5

10

10

10

10

10

10

I l.l

10

10
4

10

40

100

0.140
0.193
0.287
0.523
1.02
2.81
4.89
4.90

9.
10.
13.
16.
16.51 (max)

RMS %
Error
12.44

9.

0.

.5 .8

1.25

0.562

9.27 (max)

Life Prediction Ratio Summary


i

0.0436
0.0451
0.110
0.203
0.331
0.560

4.93 (min)
5.
6.
7.
8.

0.131

6.
7.
8.

100

da/dN (10-6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

5.82 (min)

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

2.

RMS %
Error
24.71

Figure 6.16.3.1.15
6-250

Life Prediction Ratio Summary

0.

.5

.8

1.25

2.

-\ T1-6AI-4V r
Condition/Ht: ALPHA-BETA FORGE-ANNEALED
Form: Forging
Specimen Type: CT
Orientation: LT
Stress Ratio: 0.1
Frequency: 30 Hz
(3 of 3)

AK (MPaVin)
4

- I

10

' I M'l'l

40

AK (MPaVin)
4

100

' I 'l'l'l

Environment: Lab Air R.T.;


_ Yield Strength: 100 Ksi

40

100

10

10

10

10

JO)

10"
o
\

6^10-4
\
c
_

10~

10

-o

10

10

10

10

/i,

10

i , i .i.i.

10

40

10
4

100

da/dN (10"6in/cycle)

AK (KsiVin)

40

100

da/dN (I0"6in/cycle)

AK (KsiVin)

0.00904
0.00958
0.0513
0.101
0.191
0.386

3.98 (min)
4.
5.
6.
7.
7.78 (max)

Life Prediction Ratio Summary


0.

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
30.24

'

_R

10
10

10 \

'I

-z.

Z 10

10

05

io'

10

10
10

10
\
c

10

= i ' i'ITIi ' i 'i'i'i

10

Yield Strength: 50-100 ksi


Ult. Strength:
Specimen Thk: 0.25 - 0.252 in.
Specimen Width: 1.993 - 2.01 in.
Ref: SA001

.5

.8

RMS %
Error

Life Prediction Ratio Summary


0.

1.25

Figure 6.16.3.1.15 (Concluded)


6-251

.5

.8

1.25

^ TJ-6AI-4V I
Condition/Ht: ANNEALED
Form: 6 in. Billet
Specimen Type: WOL
Orientation: LT
Stress Ratio: 0.02
Frequency: 10 - 20 Hz

Yield Strength: 123 ksi


Ult. Strength: 135 ksi
Specimen Thk: 1.25 in.
Specimen Width: 5 in.
Ref: MA003
(1 of 1)

AK (MPaVin)
4
10
40 100
_ p-, | i|i,i|
| . | T|i|
Environment: Lab Air; R.T.

AK (MPaVin)
10
40 100
llll
I ' I 'I'll

4
a
~

r=1I
10

10

10

10

10

10

10
2

io"

o
o 10
\
c

*
_

10

x>

X>

10

10

-o

XI

10

-no'2
o

_a>

o
_
6^10-4
c
|_

-5

Z10
X<

10

10

-5

-JlO >
x>

, 10

10

10

-7

10

10

III I

10

10

I , l.l.l,

10
4

10

40

10

I , 1,1 L.
4

100

da/dN (10"6in/cycle)

16.27

0.

100

da/dN (10-6in/cycle)

AK (KsiVin)

34.9
62.7
86.4
138.

Life Prediction Ratio Summary


o
i

I I I III

0.210
0.270
1.12
4.22
11.1
18.7

9.04 (min)
10.
13.
16.
20.
25.
30.
35.
40.
44.93 (max)

RMS %
Error

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


r

0.

2.

Figure 6.16.3.1.16
6-252

.5

.8

1.25

\ TI-6AI-4V h
Condition/Ht: ANNEALED
Form: 1.75 in. Extrusion
Specimen Type: CT
Orientation: LT
Frequency: 1 Hz
Environment: DIST WATER; RT

10

40

Yield Strength: 127.2 - 131.6 ksi


Ult. Strength:
Specimen Thk: 0.247 - 0.252 in.
Specimen Width: 2 - 2.008 in.
Ref: DA006;DA007

AK (MPaVin)

100

b I

10

40

100

RMS %
Error
26.52

40

100

da/dN (10"6in/cycie)
0.0230
0.0245
0.0750
0.223
0.348
0.453
0.595

3.48 (min)
3.5
4.
5.
6.
7.
8.
9.
10.
13.
14.23 (max)

0.106
0.181
0.275
0.391

0.969
2.33
7.49

21.9
37.9
57.5
102.
206.

Life Prediction Ratio Summary


CA
o
-r-

1.25

100

' I 'I'l'l

10

AK (KsiVin)

0.0411
0.0508

.5 .8

40

AK (KsiVin)

da/dN (10'6in/cycle)

5.77 (min)
6.
7.
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
46.98 (max)

10

' I M'l'l

AK (KsiVin)
AK (KsiVin)

(2 of 2)

AK (MPaVin)

2)

' I Tl'l

RMS %
Error

0.853
1.37
11.6

36.8

Life Prediction Ratio Summary


T~

29.39

Figure 6.16.3.1.17
6-253

.5

.8

1.25

\ Ti-6AI-4V r
Condition/Ht: ANNEALED
Form: 1.75 in. Extrusion
Specimen Type: CT
Orientation: LT
Frequency: 15 Hz
Environment: LAB AIR; RT

Yield Strength: 127.2 - 131.6 ksi


Ult. Strength:
Specimen Thk: 0.25 - 0.251 in.
Specimen Width: 2.001 - 2.003 in
Ref: DA006;DA007
(1 of 2)

AK (MPaVin)
1

10

40

El ' I 'I'l'l

100

I ' I Tl'l

Stress Ratio: 0.4

10

4
. I

10
lljll

40
100
I I ll<lll

Stress Ratio: 0.8

""""

10

10

-3

IQ"3

10

""""

_a>

10"2

io-

o^io"4

- -3 I

10

""*

2
10"
o
\

-3

Z10-

_i"0

10

'1

^-^

""~

10 \
u
-o

-6
10

10
_

-5

cl

10

10

-7

j*r

10

10

10

10
.-8

10~

Z. 10

10

-1
-= 10

10

10

\
a
~

(2 of 2)

AK (MPaVin)

- I , ll,l,
4

I , I,I,I,

10

40

10

100

da/dN (10'6in/cycle)

RMS 55
Error
38.93

100

0.0402
0.0453
0.0961
0.167
0.276
0.458
0.779
1.37
9.09
15.3

3.88 (min)
4.
5.

6.
7.
8.

0.142
0.235

0.371
0.572
2.07
6.55

9.
10.
13.
13.76 (max)

16.5
28.2

64.3
128.

Life Prediction Ratio Summary


o

T"

0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.0249
0.0340
0.0770

4.70 (min)
5.
6.
7.
8.
9.
10.
13.
16.
20.
25.
30.
34.29 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , 1,1,1,

" I , LI,I,

.5

.8

1.25

2.

RMS %
Error
7.41

Figure 6.16.3.1.18
6-254

Life Prediction Ratio Summary


a
i

0.

.5

.8

1.25

2.

This page intentionally left blank

6-255

\ Ti-6AI-4V I
Condition/Ht: ANNEALED
Form: 1.75 in. Extrusion
Specimen Type: CT
Orientation: L-T
Stress Ratio: 0.1
Environment: LAB AIR; RT

Yield Strength: 127.2 - 131.6 ksi


Ult. Strength:
Specimen Thk: 0.251 - 0.252 in.
Specimen Width: 2.002 - 2.006 in
Ref: DA006;DA007
(1 of 3)

AK (MPaVin)
4

10

40

(2 of 3)

AK (MPaVin)
4

100

' ' "Tl

- I

10

I I >l'l'l

40

100
A

' I 'l'l'l

Frequency: 15. Hz

-2

10

10

10
ja;

a>
10"

cj

6^10-4
\
c
_

/
-= 10"

Z 10
o

o
\

I
z

/
-=

_r10

"
m \
u

/
10

10
-6

-r: 10
10
4

10

40

- i , i,i,i,
4

100

da/dN (10"6in/cycle)

6.
7.
8.

0.339
1.33
4.92
11.6
23.6
30.0

Life Prediction Ratio Summary

0.

.5

.8

100

1.25

0.632
2.63
8.68
20.4
35.2
58.7
98.9
243.
324.

13.00 (min)
16.
20.
25.
30.
35.
40.
50.
53.58 (max)

0.154
0.229

9.
10.
13.
16.
20.
25.
29.43 (max)

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.0458
0.0477
0.0951

5.95 (min)

RMS %
Error
12.17

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i , i,I,I,

2.

RMS %
Error
5.80

Figure 6.16.3.1.19
6-256

Life Prediction Ratio Summary


r-

0.

.5

r-

.8

1.25

H TJ-6AI-4V h
Condition/Ht: ANNEALED
Form: 1.75 in. Extrusion
Specimen Type: CT
Orientation: LT
Stress Ratio: 0.1
Environment: LAB AIR; RT

Yield Strength: 127.2 - 131.6 ksi


Ult. Strength:
Specimen Thk: 0.251 - 0.252 in.
Specimen Width: 2.002 - 2.006 in
Ref: DA006;DA007
(3 of 3)

AK (MPaVin)
1

10

40

ET' 1 U'l'l

100

1 ' 1 'I'l'l

Frequency: 20. Hz

AK (MPaVin)
4

-1 10

~=

10
i

40

i i

100

i i

10"

-2

10

10

10

10
10

10
"~"

_Z u

10

_a>
u

io"

10~

10

x>

X!

10

10

10

10

10

10

-6

10

10
10

'

10 \
u

-=ho
>

o
\

Z 10

2 10

'I

o 10

-3 EI

~~
_

Q)
2

10"

1 , 1,1,1,

" 1 . I.ftl,
4 |f]

10

40

10
4

100

AK (KsiVin)

100

0.00539
0.00891
0.0317
0.0561
0.116
0.180
0.391
2.52
2.83

5.74 (min)
6.
7.
8.
9.
10.
13.
16.
16.26 (max)

RMS %
Error
21.89

40

da/dN (10-6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

10

AK (KsiVin)

Life Prediction Ratio Summary


r-

.5

RMS %
Error

Life Prediction Ratio Summary


i

^8 TJi"

0.

Figure 6.16.3.1.19 (Concluded)


6-257

.5

.8

1.25

!-

2.

j U-6AI-4V I
Condition/Ht: ANNEALED
Form: 1.75 in. Extrusion
Specimen Type: CT
Orientation: L-T
Stress Ratio: 0.8
Environment: LAB AIR; RT

Yield Strength: 127.2 - 131.6 ksi


Ult. Strength:
Specimen Thk: 0.25 - 0.253 in.
Specimen Width: 2 - 2.004 in.
Ref: DA006;DA007
(1 of 2)

AK (MPaVin)
1

b I

10

' I M'l'l

40

(2 of 2)

AK (MPaVin)
4

100

' i """

10

40

100

Frequency: 30. Hz

~= 10

10

10

10

10"

'1

10"

ZL 10

10

10

10
10

40

" J
~ 1 ift.U,
>4

RMS %
Error
80.89

0.

.8

1 , 1,1,1,
40

100

1.25

da/dN (10"6in/cycle)
0.00765
0.0133
0.0272
0.0794
0.151
0.227
0.343

3.16 (min)
3.5
4.
5.
6.
7.
8.
9.
10.
13.
13.25 (max)

Life Prediction Ratio Summary


a
.5

10

10

AK (KsiVin)

0.0294
0.0358
0.0575
0.133
0.244
0.374
0.576
0.965
1.68
8.23
10.2

10

AK (KsiVin)

da/dN (10"6in/cycle)

3.29 (min)
3.5
4.
5.
6.
7.
8.
9.
10.
13.
13.34 (max)

10 \
o
u

AK (KsiVin)

AK (KsiVin)

v x

-z.

100

o^10-4
\
c
_

RMS %
Error
21.98

Figure 6.16.3.1.20
6-258

0.572
0.998
3.82
4.07

Life Prediction Ratio Summary


a
0.

1~

r~

.5

.8

1.25

2.

-I Ti-6AI-4V r
Condition/Ht: ANNEALED
Form: 1.75 in. Extrusion
Specimen Type: CT
Orientation: TL
Frequency: 5 - 15 Hz
Environment: LAB AIR; RT

Yield Strength: 131.4 ksi


Ult. Strength:
Specimen Thk: 0.249 - 0.25 in.
Specimen Width: 2.002 - 2.006 in
Ref: DA006
(1 of 2)

AK (MPaVin)
1

10

40

I- I ' I M'l'l

(2 of 2)

AK (MPaVin)
4

100

= I

' I 'I'l'l

10

40

' I M'l'l

100

' I M'l'l
10

Stress Ratio: 0.4

10

40

100

da/dN (10"6in/cycle)

0.938
2.44
7.95
20.2
35.4
60.3

.5

.8

100

0.0500
0.0554

4.87 (min)
5.
6.
7.
8.
9.
10.
13.
16.
20.
25.
27.26 (max)

Life Prediction Ratio Summary


0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.0527
0.0706
0.135
0.222
0.336

6.63 (min)
7.
8.
9.
10.
13.
16.
20.
25.
30.
33.16 (max)

RMS %
Error
14.99

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

1.25

2.

RMS %
Error
13.61

Figure 6.16.3.1.21
6-259

0.115

0.209
0.350
0.555
0.842
2.50
6.09
14.1
28.1
38.6

Life Prediction Ratio Summary


0.

-r-

-r-

.5

.8

1.25

\ Ti-6AI-4V I
Condition/Ht: ANNEALED
Form: 1.75 in. Extrusion
Specimen Type: CT
Orientation: T-L
Frequency: 20 Hz
Environment: LAB AIR; RT

Yield Strength: 127.9 ksi


Ult. Strength:
Specimen Thk: 0.251 in.
Specimen Width: 1.998 - 2 in.
Ref: DA007
(1 of 2)

AK (MPaVin)
_ |

4
10
. | i' j-i

40
100
' | M'l'l
-1

Stress Ratio: 0.1

10

i I Tl'l

40

100

' I M'l'l

Stress Ratio: 0.8

10

10

10

-3

-3

10

10

io"2
o
\

^io"

-3 |

~"~

10

Z 10

_0J

o
o 10
c

-o

10

10
10

10

i ,i,i,i,

10

40

10

100

*
i nl i I ill
4
10

100

0.0126
0.0145
0.0331
0.0502
0.0724
0.115
0.197
0.675
2.60
2.62

Life Prediction Ratio Summary

RMS 95
Error

Life Prediction Ratio Summary


i

!-

0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

4.89 (min)
5.
6.
7.
8.
9.
10.
13.
16.
16.01 (max)

RMS %
Error
18.88

1 , 1,1,1,

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

-Jio
>

_fi|
10

10

- i , iiu

-3 I

"

-10"\

o
-a

Z. 10

_K
10

10

10

10

10

- I

10

-o

(2 of 2)

AK (MPaVin)

.5

.8

1.25

0.

2.

Figure 6.16.3.1.22
6-260

.5

.8

1.25

2.

TI-6AI-4V r
Condition/Ht: ANNEALED
Form: 1.75 in. Extrusion
Specimen Type: CT
Orientation: TL
Frequency: 15 Hz
Environment: LAB AIR; RT

Yield Strength: 127.9 ksi


Ult. Strength:
Specimen Thk: 0.25 - 0.251 in.
Specimen Width: 2.002 - 2.003 in
Ref: DA007
(1 of 2)

AK (MPaVin)
4

10

40

b I

100

RMS %
Error
16.54

61.9
93.4
162.
188.

.8

100

' I """

10

40

100

1.25

da/dN (10"6in/cycle)
0.0257
0.0323
0.0613
0.104
0.167
0.260
0.398
1.37
4.34
13.4
28.1
54.2
105.
119.

4.69 (min)
5.
6.
7.
8.
9.
10.
13.
16.
20.
25.
30.
35.
37.43 (max)

0.330
0.498
1.74
5.84
16.9
35.7

.5

AK (KsiVin)

Life Prediction Ratio Summary


0.

40

AK (KsiVin)

da/dN (10"6in/cycle)

12.19 (min)
13.
16.
20.
25.
30.
35.
40.
50.
54.07 (max)

10

' I M'l'l

AK (KsiVin)
AK (KsiVin)

(2 of 2)

AK (MPaVin)

40
100
i i i IHM

10

2.

RMS %
Error
15.11

Figure 6.16.3.1.23
6-261

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

H H-6AI-4V r
Condition/Ht: ANNEALED
Form: 1.75 in. Extrusion
Specimen Type: CT
Orientation: TL
Frequency: 1 Hz
Environment: DIST WATER; RT

Yield Strength: 127.9 - 131.4 ksi


Ult. Strength:
Specimen Thk: 0.25 - 0.251 in.
Specimen Width: 1.998 - 2.02 in.
Ref: DA007;DA006
(1 of 2)

AK (MPaVin)
4

- I

10

40

' I 'I'll

100

' 1 'ITI

Stress Ratio: 0.1

(2 of 2)

AK (MPaVin)
4

10

40

b I ' I 'I'll

100

1 ' I M'l'l

~ 10

10
-1

10
-3

10

_a>
o

10

-6
10

Jio
>
-=:
XI

^"*

II I I

10

o
\

-3 |

Z 10
\
o
"

io"2^

-5

10

10

i , i,i,i,

-8

10

10

40

100

AK (KsiVin)

RMS %
Error
12.44

9.
10.
13.
15.64 (max)

Life Prediction Ratio Summary


i

0.

.5

r-

.8

1.25

0.0591
0.102
0.175
0.341
0.523
0.737
1.02
1.43
2.04
7.00
24.8

6.
7.
8.

14.9
31.2
60.1
83.0
109.

r-

100

3.13 (min)
3.5
4.
5.

0.469
0.863
3.06
7.72

11.99 (min)
13.
16.
20.
25.
30.
35.
40.
43.11 (max)

40

da/dN (10'6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

10

AK (KsiVin)

2.

RMS %
Error
>100.0

Figure 6.16.3.1.24
6-262

Life Prediction Ratio Summary


o
n
0.

r-

-i

.5

.8

1.25

2.

\ Ti-6AI-4V h
Condition/Ht: ANNEALED
Form: 1.75 in. Extrusion
Specimen Type: CT
Orientation: T-L
Frequency: 30 Hz
Environment: LAB AIR; RT

Yield Strength: 127.9 ksi


Ult. Strength:
Specimen Thk: 0.251 in.
Specimen Width: 2 in.
Ref: DA007
(1 of 1)

AK (MPaVin)
4

_ I

10

1 I ljTl

40

1 1

AK (MPaVin)
1

100

PH

-i

4
10
pr-ii I i |i|i|

40
I

100

I 11 III
TT

10

Stress Ratio: 0.8

10
10

10

10

10

:
10

10

io"2

6^10"+
\
c
_

5-10-4

-3i

-3 I

10

10

Z10

io"\
O

10

10

10

10

mr

-7

10

10

10

1 , 1,1,1,

~ 1 , 1,1,1,
4

10

10

10

40

10

100

da/dN (10"6in/cycle)

Life Prediction Ratio Summary


i

0.

da/dN (10"6in/cycle)

AK (KsiVin)

0.0646
0.0765
0.135
0.221
0.350
0.552
0.872
3.62
15.2

4.75 (min)
5.
6.
7.
8.
9.
10.
13.
14.97 (max)

RMS %
Error
12.09

i 11in
40
100

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i i 11in
4
10

.5

.8

-1--

1.25

2.

RMS %
Error

Life Prediction Ratio Summary


i

0.

Figure 6.16.3.1.25
6-263

.5

.8

1.25

2.

Ti-6AI-4V 1
Condition/Ht: ANNEALED
Form: 1.75 in. Extrusion
Specimen Type: CCP (max load specified)
Orientation: LT
Frequency: 5 Hz
Environment: LAB AIR; RT
(1 of 1)

AK (MPaVin)
4

10

Yield Strength: 131.6 ksi


Ult. Strength:
Specimen Thk: 0.198 in.
Specimen Width: 4.009 in.
Ref: DA006

40

AK (MPaVin)
4

100

= I

10

' I M'l'l

40

100

' I Tl'l

10
10
-3

10

<D

2
10" o
o
\

o
^10"4
c

10~

^-y

-z.

10

m
o

i ~
'\
o
X

10
10

10
10
10
4

10

40

100

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)

0.

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.260
0.414

0.957
2.04
7.29
23.4
32.8
51.0
53.6

Life Prediction Ratio Summary


i

40

0.0720
0.129

7.42 (min)
8.
9.
10.
13.
16.
20.
25.
30.
35.
35.32 (max)

RMS %
Error
21.79

10

AK (KsiVin)

.5

.8

1.25

RMS %
Error

2.

Figure 6.16.3.1.26
6-264

Life Prediction Ratio Summary


i

.5

.8

1.25

J T;

4
10
1 | l|l|'|

(1

40
100
' | 'I'l'l

of 2)

-L

- I

10

40

I rn

100

| 'i'i'i

-1

~~*~ 10

ID"3

IQ"3

ZIG"5
T3
\
O
~
-6
10

io"2

QJ

io"2

0)

o
6^10-4

10 J,

ZIG"5

10 \

\
a
" "6
10

-z.
TJ

-3|

10 JE,

10 >
o
"U

-5

-5

in"8

10

-6
10

r I , I .l.l.
1

I , I, LI,

10

40

10"7

10""

-6

10

~ 1 , I.I.I.
1

100

da/dN (10"6in/cycle)

9.25 (min)
10.
13.
16.
20.
25.
30.
35.
40.
42.62 (max)

RMS %
Error
7.79

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.196
0.375
2.19
6.12
14.3
28.7
49.0
81.0
130.
159.

Life Prediction Ratio Summary


m
0.

I , l.l.l,

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

z.

10
10~7

10"2

10

-a
10

Stress Ratio: 0.8

-1

_c

10"2

a>
o

(2 of 2)

AK (MPaVin)
1

10
,

Stress Ratio: 0.1

Yield Strength: 131.7 ksi


Ult. Strength:
Specimen Thk: 0.245 - 0.246 in.
Specimen Width: 2.007 - 2.009 in.
Ref: DA006

AK (MPaVin)
-

A\l

Condition/Ht: ANNEALED
Form: 3 in. Forging
Specimen Type: CT
Orientation: LT
Frequency: 1 Hz
Environment: DIST WATER; RT

cAI

.5

.8

1.25

2.

RMS %
Error

Life Prediction Ratio Summary


0.

Figure 6.16.3.1.27
6-265

.5

.8

1.25

2.

^ Ti-6AI-4V r
Condition/Ht: ANNEALED
Form: 3 in. Forging
Specimen Type: CT
Orientation: LT
Stress Ratio: 0.1
Environment: LAB AIR; RT

Yield Strength: 131.7 - 132.3 ksi


Ult. Strength:
Specimen Thk: 0.248 - 0.251 in.
Specimen Width: 2.005 - 2.007 in
Ref: DA006;DA007
(1 of 3)

AK (MPaVin)
4

10

40

_ I 1 I llllll
1
- Frequency: 5. Hz

100

1 1 illlll

J.
~

(2 of 3)

AK (MPaVin)
4

10

- I ' I Tl'l

40

100

-1

I ' I H'l'l

Frequency: 15. Hz

10

10

10

10

10

10

10
~*

io"

2 <0

~~"
_Q3

10"

6^10-

o 10
c

_
-5

10

XI

10

10

-7

:
10

i , i.i.i,
40

.-8

10

100

ra

.8

100

1.25

1.04
2.16
5.72
11.1
23.2
44.6
79.1
161.
417.

11.75 (min)
13.
16.
20.
25.
30.
35.
40.
47.45 (max)

0.0593

.5

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.0818
0.149
0.294
1.82
5.13
9.53
21.1
43.2
43.3

Life Prediction Ratio Summary


0.

10

AK (KsiVin)

da/dN (10"6in/cycle)

7.19 (min)
8.
9.
10.
13.
16.
20.
25.
30.
30.03 (max)

i . i. t,i,

- i , i, i.i,

AK (KsiVin)

RMS %
Error
14.91

XI

10

10

AK (KsiVin)

m" ^
u

10

i , i,i,i,

10

10

10

T3

10

'I

^-^

10

10

10

\
10"

RMS %
Error
4.13

Figure 6.16.3.1.28
6-266

Life Prediction Ratio Summary


a
i

0.

.5

.8

1.25

\ Ti-6AI-4V h
Condition/Ht: ANNEALED
Form: 3 in. Forging
Specimen Type: CT
Orientation: L-T
Stress Ratio: 0.1
Environment: LAB AIR; RT

Yield Strength: 131.7 - 132.3 ksi


Ult. Strength:
Specimen Thk: 0.248 - 0.251 in.
Specimen Width: 2.005 - 2.007 in
Ref: DA006;DA007
(3 of 3)

AK (MPaVin)
1

-IM

10

AK (MPaVin)
4

40
100
-lI I I I MM

M'l'ir

10

40
100
i I i I HU

I 'I'l'l

10

10

Frequency: 20. Hz

10

10
-3

10

6^10-4

,0*1
"O

10

-s
-

-i"0

10

-6

10

10
10
10
10
4

10

40

da/dN (I0"6in/cycle)

20.95

Life Prediction Ratio Summary

0.

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.0189
0.0282
0.0714
0.175
0.376
1.77
6.20
8.20

6.51 (min)
7.
8.
9.
10.
13.
16.
17.19 (max)

RMS 95
Error

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

LI

i i 1111

100

.5

.8

RMS %
Error

Life Prediction Ratio Summary


i

0.

1.25

Figure 6.16.3.1.28 (Concluded)


6-267

.5 .8

1.25

1 Ti-6AI-4V I
Condition/Ht: ANNEALED
Form: 3 in. Forging
Specimen Type: CT
Orientation: LT
Stress Ratio: 0.4
Environment: LAB AIR; RT

Yield Strength: 131.7 - 132.3 ksi


Ult. Strength:
Specimen Thk: 0.249 in.
Specimen Width: 2.005 - 2.008 in
Ref: DA006;DA007
(1 of 2)

AK (MPaVin)
4

10

40

100

~ 10

Frequency: 10. Hz

(2 of 2)

AK (MPaVin)
10

40

100

Frequency: 20. Hz

-2

10

10

10

10

10

10
_a>
o

10

:
z 10

-I

10

T3

-l"0

10

-r: 10

XI

_c

"O

_c -

10

10

10

10

jJT

10

10

10

10

10

io"2

O-10-4
c
_

10

"O

.22
o

I , I,I,I,

~ I , I,I,I,
4

10

40

I , Irfl.l,

10

100

da/dN (10"6in/cycle)

1.32
3.82
7.65

16.3
37.2

Life Prediction Ratio Summary


i

.5

.8

1.25

0.0144
0.0215
0.0546
0.132

4.56 (min)
5.
6.
7.
8.
9.
10.
13.
16.
20.
25.
30.
33.23 (max)

0.177
0.381
0.755

9.
10.
13.
16.
20.
24.31 (max)

0.

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.0531
0.0537
0.0847

4.90 (min)

5.
6.
7.
8.

RMS %
Error
17.37

:
40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I ,

10

2.

RMS %
Error
14.81

Figure 6.16.3.1.29
6-268

0.293
0.591
1.0S
4.16

9.07
17.6
38.4
83.1
121.

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

H Ti-AI-^i/^ 'I r
Condition/Ht: ANNEALED
Form: 3 in. Forging
Specimen Type: CT
Orientation: LT
Stress Ratio: 0.8
Environment: LAB AIR; RT

Yield Strength: 131.7 - 132.3 ksi


Ult. Strength:
Specimen Thk: 0.248 - 0.249 in.
Specimen Width: 2.005 - 2.006 in.
Ref: DA006;DA007

AK (MPaVin)
4

10

'

40

- I i I Tl'l

of 2)

1
10
_

(2 of 2)

AK (MPaVin)

100

I ' I M'l'l j

Frequency: 15. Hz
""

ID"2

(1

10

- I i I i |T!

40

100

' 1 M'l'l

io"2
10

10

a>
o

10
10

-3l
io vE

~'

2 10"5

\
o

T3

u 10
\
c

Z10"5

<o

io'2

a;
o

v_^

io"3

'T
2
io"
-3|
10 E

o
"

10 >
o
"D

-6
10
-5

-5

10

10

io"7

10

JP
-

*&

~ I 71,1,1,

irT8
1

I , LI,!.

10

40

io"7

Br

m"8

da/dN (10"6in/cycle)

40

100

da/dN (10~6in/cycle)

AK (KsiVin)

0.0422
0.0253
0.0305
0.0472
0.0687
0.105

Life Prediction Ratio Summary


0.

I , LI,I,

10

AK (KsiVin)

2.83 (min)
3.
3.5
4.
5.
5.48 (max)

RMS %
Error
8.80

10

^ 1 , 1,1,1,
1

100

-6

AK (KsiVin)
AK (KsiVin)

10

Frequency: 30. Hz

-1

io-3

-1

.5

.8

1.25

2.

RMS %
Error

Life Prediction Ratio Summary


0.

Figure 6.16.3.1.30
6-269

.5

.8

1.25

2.

^ TJ-6AI-4V r
Condition/Ht: ANNEALED
Form: 3 in. Forging
Specimen Type: CT
Orientation: TL
Frequency: 1 Hz
Environment: DIST WATER; RT

Yield Strength: 140.1 - 144.9 ksi


Ult. Strength:
Specimen Thk: 0.248 - 0.25 in.
Specimen Width: 2 - 2.006 in.
Ref: DA006;DA007
(1 of 2)

AK (MPcVin)
4

- I

10

40

i I M'l'l

100

' I 'l'l'l

- I

10

Stress Ratio: 0.1

10

40

100

' I 'l'l'l

Stress Ratio: 0.8

10

-3

10

10

io"2

6-10-

-6

10

~~

-= 10

2 10

\
o

"

""

10 JE,

z
-J10
>

z. 10

6-10-4

-3 |

J2

o
\

"

10

' I M'l'l

10

10

\
o

(2 of 2)

AK (MPaVin)

10 >
o
a

-6
10

-5

10

10

-7

10

10

10

10

10

I , I,I,I,
4

I , l.l.l,

10

40

.-8

10

" I , I,I,I,
4

100

da/dN (10"6in/cycle)

RMS %
Error
13.38

0.

.8

1.25

0.504
0.543
1.22
8.14
15.8
12.8
9.26
9.63
17.5
33.1

3.40 (min)
3.5
4.
5.
6.
7.
8.
9.
10.
11.28 (max)

Life Prediction Ratio Summary


o
.5

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.0630
0.145
0.326
0.630
1.09
1.76
2.64
6.96
14.1
28.5
53.8
85.7
130.
226.
297.

4.17 (min)
5.
6.
7.
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
41.96 (max)

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , I,I,I,

10

RMS %
Error
23.12

Figure 6.16.3.1.31
6-270

Life Prediction Ratio Summary


i

0.

.5

-i

.8

1.25

2.

This page intentionally left blank

6-271

-\ Ti-6AI-4V r
Condition/Ht: ANNEALED
Form: 3 in. Forging
Specimen Type: CT
Orientation: T-L
Stress Ratio: 0.1
Environment: LAB AIR; RT

Yield Strength: 140.1 - 144.9 ksi


Ult. Strength:
Specimen Thk: 0.249 0.251 in.
Specimen Width: 2.003 - 2.008 in
Ref: DA006;DA007
(1 of 3)

AK (MPaVin)
4
1

10

I 'I'l'l

40

100

1 ' I Tl'l

Frequency: 5. Hz

(2 of 3)

AK (MPaVin)
4

- I
10

10

i I MM'I

40

100

' I 'I'l'l

Frequency: 10. Hz

-1
-r:

10

10

10
:
-3

IQ"3

10

5^io-4
c
l_

-3 I
E

J
-z 10" E

Z 10

10
o
~

10

-6
10

10
10

10
-7

10

10

'

I i 11 li

10

10

i i i i n

40

^P

10
10

"

100

, I,I,I,
40
100

da/dN (10"6in/cycle)

AK (KsiVin)

6.86
13.1
27.8
65.1

17.23 (min)
20.
25.
29.98 (max)

Life Prediction Ratio Summary


0.

-6

10

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

-=

, I,I,I,
4
10

AK (KsiVin)

RMS %
Error
5.66

10

10

o
o 10

.5

.8

RMS %
Error

Life Prediction Ratio Summary


.5

1.25

Figure 6.16.3.1.32
6-272

.8

1.25

2.

\ T1-6AI-4V r
Condition/Ht: ANNEALED
Form: 3 in. Forging
Specimen Type: CT
Orientation: T-L
Stress Ratio: 0.1
Environment: LAB AIR; RT

Yield Strength: 140.1 - 144.9 ksi


Ult. Strength:
Specimen Thk: 0.249 - 0.251 in.
Specimen Width: 2.003 - 2.008 in
Ref: DA006;DA007
(3 of 3)

AK (MPaVin)
4

10

AK (MPaVin)
4

40
100
I I i I i Ml

' I Tl'l

- I

10

' I M'l'l

40

100

' I M'l'l

Frequency: 20. Hz

10

10

10

10

_a)
o
^

o 10
\
c

6^10-4

io"2

\
-3 |

10

2 10

10

-1<T\
o
T>
10

10

10
10

10

10
10

10

10

40

100

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)

100

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


0.

40

0.0283
0.0528
0.105
0.204
0.373
0.646
2.41
5.91
12.1
21.1
36.1
68.0
134.
231.

5.08 (min)
6.
7.
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
44.11 (max)

RMS %
Error
37.27

10

AK (KsiVin)

.5

.8

RMS %
Error

Life Prediction Ratio Summary

0.

1.25

Figure 6.16.3.1.32 (Concluded)


6-273

.5

.8

1.25

I TI-6AI-4V h
Condition/Ht: ANNEALED
Form: 3 in. Forging
Specimen Type: CT
Orientation: TL
Stress Ratio: 0.4
Environment: LAB AIR; RT

Yield Strength: 140.1 - 144.9 ksi


Ult. Strength:
Specimen Thk: 0.246 - 0.251 in.
Specimen Width: 2.005 - 2.006 in
Ref: DA006;DA007
(1 of 2)

AK (MPaVin)
4
10
40 100
1
I I l I l i M
-IN 'I'l'
Frequency: 10. Hz

(2 of 2)

AK (MPaVin)
4
10
40 100

1
- I

I I >lll>l

' I 'I'll

- Frequency: 20. Hz

10

10

-2

-2

10

10

__

io-3

10

v
o
o 10

o
o 10

2
o
10"
u
\

-= 10"

z. 10

Z10
a

\
o
"

'

o
-6
10

i "n

'\
u
D

rfi

10
~

-5

fflfi

10

10

10

10
10

10
4

10
40
AK (KsiVin)

AK (KsiVin)

100

100

0.0279
0.0508

4.58 (min)
5.
6.
7.
8.
9.
10.
13.
16.
20.
25.
28.75 (max)

0.0461
0.0994
0.224
0.480
0.923
1.57
2.41

5.71
9.58
18.6
31.7

.5 .8

40

da/dN (10_6in/cycle)

AK (KsiVin)

0.0498

Life Prediction Ratio Summary


0.

1 , 1,1,1,

10

AK (KsiVin)

da/dN (10~6in/cycle)

3.83 (min)
4.
5.
6.
7.
8.
9.
10.
13.
16.
20.
22.36 (max)

RMS %
Error
12.79

- i , m,i,

1.25

RMS %
Error
37.04

Figure 6.16.3.1.33
6-274

0.149
0.325

0.589
0.949
1.41
3.56
7.37
17.3
47.3

98.8

Life Prediction Ratio Summary


,
0.

.5 .8

1.25

This page intentionally left blank

6-275

-i -6AI-4V h
Condition/Ht: ANNEALED
Form: 3 in. Forging
Specimen Type: CT
Orientation: TL
Stress Ratio: 0.8
Environment: LAB AIR; RT

Yield Strength: 140.1 - 144.9 ksi


Ult. Strength:
Specimen Thk: 0.249 - 0.25 in.
Specimen Width: 2.004 - 2.008 in
Ref: DA006;DA007
(1 of 3)

AK (MPaVin)
4

- i ' i

40
100
T
1
I
I
I
l|l|
M'l'ir

10

Frequency: 15. Hz

(2 of 3)

AK (MPaVin)

10

10

- i i Ti'irI

40

100

' I 'I'M

Frequency: 10. Hz

10

-2

10

10

10

10
10

IQ"3

^1 u

_CJ

fri o-4
10

_c

10

o
_
o^10-4

T>

-3 |

_
10

10

-5

10

10
XI

X)

_. -

10

10

10

10

JS_

10

10

10

10

I i.l.i.

10

10

10

40

100

da/dN (10'6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


0.

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.0256
0.0369
0.0633
0.105
0.233
0.425
0.729
1.24
1.73
1.76

2.61 (min)
3.
3.5
4.
5.
6.
7.
8.
9.
9.23 (max)

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
7.47

.5

.8

RMS %
Error

Life Prediction Ratio Summary


i

0.

1.25

Figure 6.16.3.1.34
6-276

.5

r-

.8

1.25

\ TI-6AI-4V h
Condition/Ht: ANNEALED
Form: 3 in. Forging
Specimen Type: CT
Orientation: TL
Stress Ratio: 0.8
Environment: LAB AIR; RT

Yield Strength: 140.1 - 144.9 ksi


Ult. Strength:
Specimen Thk: 0.249 - 0.25 in.
Specimen Width: 2.004 - 2.008 in
Ref: DA006;DA007
(3 of 3)

AK (MPaVin)
4

- I

10

' I 'I'l'l

40

AK (MPaVin)
4

100
1

' I M'l'l

= I

Frequency: 20. Hz

10

' I 'I'l'l

40

100

' I 'I'l'l

10

10

10
10

10

10" ^
o

_QJ
O

^10"4

10

o
"

10"

-6
10

_A"0

10

XI

10

10

10
10

10

.-8

10

'I

'
-z.
in" ^

2L 10

10

10"
c>
\

-3 iz

-5

-=

10

O^O"4

1 , i , 1,1,

~ 1 , 1,1,1,
4

10

10

10

40

10
4

100

da/dN (10'6in/cycle)

AK (KsiVin)

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.592
0.986
1.26
2.22
6.32
9.59

Life Prediction Ratio Summary


0.

40

0.128
0.254

4.06 (min)
5.
6.
7.
8.
9.
10.
10.53 (max)

RMS %
Error
16.59

10

AK (KsiVin)

AK (KsiVin)

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary

0.

2.

Figure 6.16.3.1.34 (Concluded)


6-277

.5

.8

1.25

\ Ti-6AI-4V I
Condition/Ht: ANNEALED
Form: 3 in. Forging
Specimen Type: CCP (max load specified)
Orientation: LT
Frequency: 5 Hz
Environment: LAB AIR; RT
(1 of 1)

AK (MPaVin)
4

10

- T ' I 'I'l'l

40

Yield Strength: 131.7 ksi


Ult. Strength:
Specimen Thk: 0.205 in.
Specimen Width: 4.018 in.
Ref: DA006

AK (MPaVin)
4

100
a

' I 'l'l'l

Stress Ratio: -1.0

- I

'I 'I'l'l

40

100

' I 'I'l'l

-=
10

10

10

10

-3

IQ'3

10

2
10"

10

fci oc

\
o

-s

10

T3

10

-6
10
10

10

10

10

l , l,l,l,

~ I , I,l,l,
4

- 10'\
o

10

.-8

-3 |

10

Z 10

10

10

o
-10-4

10

10

10

40

10

100

0.

100

da/dN (lO^in/cycle)

0.520
0.868
2.45

4.89
10.3
21.9
36.5
37.0

Life Prediction Ratio Summary


a
,

40

0.0501
0.110
0.268

6.33 (min)
7.
8.
9.
10.
13.
16.
20.
25.
30.
30.15 (max)

RMS %
Error
11.51

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

10

AK (KsiVin)

AK (KsiVin)

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


i

0.

2.
Figure 6.16.3.1.35
6-278

.5

1-i

.8

1.25

2.

^ Ti-6AI-4V
Condition/Ht: ANNEALED AT 1375F 3HRS AC
Form: 2.75 in. Plate
Specimen Type: WOL
Orientation: LT
Frequency: 10 - 20 Hz
Environment: LAB AIR; RT

10

Yield Strength: 129 ksi


Ult. Strength: 139 ksi
Specimen Thk: 1.25 in.
Specimen Width: 5 in.
Ref: MA003

(1 of 1)

AK (MPaVin)

AK (MPaVin)
4
10
I MMIII

40
100
i I i I mi

- I ' I 'IT

40

100

I 'I'l'l
10

- Stress Ratio: 0.02


10

10

10
o

o
o^10-4
10

"a

10

Jio >
T3

10
-5
10

10
10

10
4

10

40

100

AK (KsiVin)

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

0.141
0.162

8.52 (min)
9.
10.
13.
16.
20.
25.
30.
35.
40.
42.37 (max)

RMS %
Error
13.73

I M I III
40
100

I Mill
4
10

0.249
1.26
4.62
11.0
19.8
37.9
64.4
122.
217.

Life Prediction Ratio Summary


.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


0.

2.

Figure 6.16.3.1.36
6-279

.5

.8

1.25

] TJ-6AI-4V
WELDMENT (HAZ)

Condition/Ht: AS WELDED E.B.


Form: Weldment
Specimen Type: CT
Orientation: TL
Frequency: 10 Hz
Environment: LAB AIR; RT

Yield Strength:
Ult. Strength:
Specimen Thk: 1 in.
Specimen Width: 2 in.
Ref: 88144
(1 of 1)

AK (MPaVin)
4

- I

10

40

I I 'I'I'I

AK (MPaVin)
1

100
a

' I 'I'I'I

10

- I ' I 'I'I'I

40

100

I ' I 'I'I'I

10

Stress Ratio: 0.1


-2

10

10

10

10

10

10

io"3

io"

10"

|_

io"

O-10\

10

10 ^E

Z. 10

o _K I
10

X)

10~\
o

\
o
"o

(0

o
\

=1

"--'

-z.

Z 10"

T3

-=:

_B I
10

i ~
\
u
x>

-5

10

10

-7

10

10

-= 10

10
10

-1

~lil ilili
4

i ,I,I,I,

10

40

10

- i , i.i.i,
4

100

da/dN (10"6in/cycle)

100

da/dN (10"6in/cycle)

AK (KsiVin)

1.98
2.50
6.52
13.2
24.7
50.2
52.9

15.35 (min)
16.
20.
25.
30.
35.
35.34- (max)

RMS 35
Error
7.63

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

1 , Ml

10

Life Prediction Ratio Summary


i

.5

.8

RMS %
Error

1.25

Figure 6.16.3.1.37
6-280

Life Prediction Ratio Summary


i

.5

.8

1.25

\ Ti-6AI-4V h

(1 of 1)

AK (MPcVin)
1

10

40

- I ' I M'l'l

WELDMENT (WELD ZONE)


Yield Strength:
Ult. Strength:
Specimen Thk: 1 in.
Specimen Width: 2 in.
Ref: 88144

Condition/Ht: AS WELDED E.B.


Form: Weldment
Specimen Type: CT
Orientation: T-L
Frequency: 10 Hz
Environment: LAB AIR; RT

AK (MPaVin)
1

100

10

tl'l M'l'l

1 ' I Tl'l

40

100

1 ' I M'l'l

10

Stress Ratio: 0.1

10

10

10

10

10
IQ"3

10

^10"

10

io"2

_a)

o
_
6^10-4
c

o
\

-3 |

10

-5

10

T3

10

"o

10

10

-o

10

_e 10
10

10
10

10

10

10
10rr
1

I,U.I
4

, I,I,I

10

40

10

I l.l li!
4

100

da/dN (10"6in/cycle)

0.

100

da/dN (I0"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


i

40

0.700
5.94
18.0
17.4

16.39 (min)
20.
25.
25.65 (max)

RMS %
Error
40.92

10

I ' I I ll

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'

.5

.8

1.25

RMS S5
Error

Life Prediction Ratio Summary


i

0.

2.

Figure 6.16.3.1.38
6-281

.5

.8

1.25

i-'

2.

-I TI-6AI-4V r
Condition/Ht: BA
Form: 0.05 in. Sheet
Specimen Type: CT
Orientation:
Frequency: 10 Hz
Environment: LAB AIR; RT

Yield Strength: 130 ksi


Ult. Strength:
Specimen Thk: 0.05 in.
Specimen Width: 3.94 in.
Ref: NL001
(1 of 1)

AK (MPaVin)
1

10

40

AK (MPaVin)
1

100

- I

10

' I M'l'l

40

100

' I 'I'l'l

10

Stress Ratio: 0.1

10

10

10

10

-3

10

10

o 10
\
c

o
5^io-4
c
_

10

io"2^
o

10

10

jM

"u

10

_e

"a

-
10

10

10

10

-7

10

10

10

10

10

I , I,I,I,

I , I ,l,l,

40

10

10
4

100

da/dN (10"6in/cycle)

AK (KsiVin)

100

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


o

0.

40

1.45
1.91
2.47
3.09
3.81
4.66
8.43
15.4
24.2

5.13 (min)
6.
7.
8.
9.
10.
13.
16.
18.19 (max)

RMS %
Error
16.43

10

AK (KsiVin)

AK (KsiVin)

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


0.

2.

Figure 6.16.3.1.39
6-282

.5

.8

1.25

This page intentionally left blank

6-283

\ Ti-6AI-4V I
Condition/Ht: BA
Form: 0.05 in. Sheet
Specimen Type: CCP (max load specified)
Orientation:
Frequency: 10 Hz
Environment: LAB AIR; RT
(1 of 3)

AK (MPaVin)
4
10
i I i I MM

Yield Strength: 130 ksi


Ult. Strength:
Specimen Thk: 0.05 in.
Specimen Width: 3.15 in.
Ref: NL001
(2 of 3)

AK (MPaVin)

40
100
1MM MM

4
10
I I <lllll

40
100
I I llllll

-1

Stress Ratio: 0.3

-= 10

10

10

10
_OJ

Sio'4
c

-=

10

z. 10

10

.-6

o
T3

10

10

10

10
10
4

10

40

100

i , i,i,i,

i , i.i.i.

40

RMS %
Error
8.49

r~

.5

.8

1.25

11.1
14.9
26.3
41.6
62.4
90.5
211.
732.

17.87 (min)
20.
25.
30.
35.
40.
50.
59.74 (max)

1.83
1.84
4.90
8.75
14.4
22.5
32.5
45.8
63.9
122.
234.
485.
536.

Life Prediction Ratio Summary


0.

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

9.98 (min)
10.
13.
16.
20.
25.
30.
35.
40.
50.
60.
70.
71.28 (max)

100

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

RMS %
Error
7.35

Figure 6.16.3.1.40
6-284

Life Prediction Ratio Summary


!-

0.

.5

.8

1.25

2.

^ Ti-6A!-4V
Condition/Ht: BA
Form: 0.05 in. Sheet
Specimen Type: CCP (max load specified)

Yield Strength: 130 ksi


Ult. Strength:
Specimen Thk: 0.05 in.
Specimen Width: 3.15 in.
Ref: NL001

Orientation:
Frequency: 10 Hz
Environment: LAB AIR; RT
(3 of 3)

AK (MPaVin)
4

10

AK (MPaVin)
4
10
! i i mi

40
100
i I i I HU

40

100

I I I I'MI
10

-2
10

10
-3

10
_0)
U

u
\

o^10-4

-3 |

10

10
o

_^T3
10

10
10
10
10
.-8

10
4

10

40

'

100

da/dN (10"6in/cycle)

Life Prediction Ratio Summary


i

0.

da/dN (10"6in/cycle)

AK (KsiVin)

2.63
3.87
8.88
15.3
26.4
50.5
134
515.

9.03 (min)
10.
13.
16.
20.
25.
30.
33.00 (max)

RMS %
Error
5.36

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I I I I III
40
100

I I III!

.5

.8

RMS %
Error

Life Prediction Ratio Summary

1.25

Figure 6.16.3.1.40 (Concluded)


6-285

.5

.8

1.25

i-'

2.

\ Ti-6AI-4V r
Condition/Ht: BA
Form: 0.76 - 2.79 in. Plate
Specimen Type: CT
Orientation: L-T
Frequency: 6 Hz
Environment: DRY AIR; RT

Yield Strength: 116.3 ksi


Ult. Strength: 125.7 ksi
Specimen Thk: 0.747 - 0.762 in.
Specimen Width: 4.993 - 5.008 in
Ref: 88575
(1 of 3)

AK (MPaVin)
4

10

40

100

10

40

100

RMS %
Error
32.89

0.

10

40

100

da/dN (10_6in/cycle)
0.265
0.290
1.73
4.79
10.1
18.3
31.9
52.9
79.6

9.89 (min)
10.
13.
16.
20.
25.
30.
35.
39.92 (max)

0.0896

0.0896
0.107
0.152
0.607
2.29
8.39
19.8

31.0
47.4
78.6
111.
108.

Life Prediction Ratio Summary

o
i

100

I ' I 'IT'

AK (KsiVin)

da/dN (10"6in/cycle)

7.64 (min)
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
50.
50.68 (max)

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

b I ' I 'I'l'l

' I I Ml

(2 of 3)

AK (MPaVin)

.5

.8

1.25

2.

RMS %
Error
10.64

Figure 6.16.3.1.41
6-286

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

T1-6AI-4V r
Condition/Ht: BA
Form: 0.76 - 2.79 in. Plate
Specimen Type: CT
Orientation: LT
Frequency: 6 Hz
Environment: DRY AIR; RT

Yield Strength: 116.3 ksi


Ult. Strength: 125.7 ksi
Specimen Thk: 0.747 - 0.762 in.
Specimen Width: 4.993 - 5.008 in
Ref: 88575
(3 of 3)

AK (MPaVin)
4

- I

10

I 'I'l'l

40

AK (MPaVin)
1

100

-1

' 1 'I'l'l

Stress Ratio: 0.5

>- I

10

40

' I 'I'l'lI

100

' I 'I'l'l

-2

10

10

10

10

10

10

10
J
o

2 u

io"

i o-4
c

(J

6^10-4

_
:

,o-I

10

10
10

T3

10

10

XI

10

10

10

10

10

10

10

10
-8

10

, 1,1,1,
4

10

, 1,1,1,
40

10

100

i i i nn
4
10

da/dN (I0"6in/cycle)

Life Prediction Ratio Summary


a
T

0.

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.428
0.541
0.800
1.15
2.86
5.76
11.4
20.2
33.0
58.5
75.9

7.43 (min)
8.
9.
10.
13.
16.
20.
25.
30.
35.
36.97 (max)

RMS %
Error
19.61

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I I I llll

.5

-i

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


i

0.

2.

Figure 6.16.3.1.41 (Concluded)


6-287

.5

.8

1.25

2.

i Ti-6AI-4V h
Condition/Ht: BA
Form: 2.25 in. Plate
Specimen Type: CT
Orientation: LT
Frequency: 0.1 Hz
Environment: H.H.A.; RT

Yield Strength: 117 ksi


Ult. Strength: 129.4 ksi
Specimen Thk: 0.749 - 0.753 in.
Specimen Width: 5.009 - 5.013 in
Ref: GD007
(1 of 3)

AK (MPaVin)
4

- I

10

40

I I I'l'l

100
1

' I 'l'l'l

10

Stress Ratio: 0.1


-2

10

40

I | 'I'l'l

100

' | 'I'l'l

-L

Stress Ratio: 0.3

-3

-1

10

10

10
-2 -r.
10" y

6^10-+
_
:

10"' E

Z 10
-O

10

10

(2 of 3)

AK (MPaVin)

_c
.-6

0)

o
o 10

*
_

-J,o>

-r: 10"

' '
z.

m" ^
u
D

_K I
10

""""

10

-o

Z 10

10

QJ

10"

10

:
10

II I I

10

-= 10

10

.-8

10

10

i 1 i 1 i li
40

10

100

i I i I Hi
4
10

da/dN (10"6in/cycle)

60.
66.20 (max)

RMS %
Error

17.91

r~

-r-

.5

.8

0.464
1.13
3.17
9.28
23.4

10.82 (min)
13.

16.
20.
25.
30.
35.
40.

39.1
52.2

86.6
210.

48.80 (max)

Life Prediction Ratio Summary


0.

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.891
0.881
1.25
3.75
13.0
27.4
42.3
59.3
112.
217.
454.

12.84 (min)
13.
16.
20.
25.
30.
35.
40.
50.

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

1 , 1,1,1,

1.25

RMS %
Error
11.30

Figure 6.16.3.1.42
6-288

Life Prediction Ratio Summary


a
0.

.5

.8

1.25

-I Ti-6AI-4V
Condition/Ht: BA
Form: 2.25 in. Plate
Specimen Type: CT
Orientation: L-T
Frequency: 0.1 Hz
Environment: H.H.A.; RT

Yield Strength: 117 ksi


Ult. Strength: 129.4 ksi
Specimen Thk: 0.749 - 0.753 in.
Specimen Width: 5.009 - 5.013 in
Ref: GD007
(3 of 3)

AK (MPaVin)
4

10

40
i

= I ' I 'IT

AK (MPaVin)
1

100

I l I M'l

10

40

100

I I I 11II

YV

' I TIM

Stress Ratio: 0.5

10

10

10
10
o
u 10

-3 |

10

10
10

T3

10
10
10

10
10
4

10

40

100

1.37
1.68
3.80
11.7
28.3
43.9
76.9
189.
1000.
1010.

Life Prediction Ratio Summary


0.

40

da/dN (10'6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

10.92 (min)
13.
16.
20.
25.
30.
35.
4-0.
50.
50.10 (max)

RMS %
Error
16.42

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

LLL

i 111in

i i 11in

100

.5

.8

RMS %
Error

Life Prediction Ratio Summary


i

0.

1.25

Figure 6.16.3.1.42 (Concluded)


6-289

.5

.8

1.25

i-'

2.

1 T1-6AI-4V I
Condition/Ht: BA
Form: 0.75 - 0.76 in. Plate
Specimen Type: CT
Orientation: L-T
Frequency: 1 Hz
Environment: S.T.W.; RT

Yield Strength: 116.3 ksi


Ult. Strength: 125.7 ksi
Specimen Thk: 0.746 - 0.751 in.
Specimen Width: 4.986 - 5.019 in
Ref: 88575
(1 of 2)

AK (MPaVin)
4

- I

10

40

' I 'I'l'l

10

10
o
o 10

zio
10

10

10

' I M'l'l

JP
Jr
m

1 , 1,1,1,

10

40

10
o

o
o 10

10'3E

10
10

-5

10
-7

10

10

10

10

1.1,1.1
4

11.0
30.0
50.1
69.1
89.9
161.
286.

.5

.8

1.25

100

53.9
61.7
87.4
114.
139.

24.08 (min)
25.
30.
35.
36.06 (max)

Life Prediction Ratio Summary


i

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.326
0.735
2.87

59.09 (max)

I.I.I.

10

AK (KsiVin)

da/dN (10"6in/cycle)

16.
20.
25.
30.
35.
40.
50.

10

100

11.43 (min)
13.

10

10

10

0.

100

' I 'I'l'l

10

AK (KsiVin)

RMS %
Error
18.47

40

Stress Ratio: 0.5

AK (KsiVin)

10

I 'I'l'l

-zz

-2
io
o
-3 I

" I , U,l,

_L

-zz 10

100

Stress Ratio: 0.1

(2 of 2)

AK (MPaVin)

2.

RMS %
Error
2.55

Figure 6.16.3.1.43
6-290

Life Prediction Ratio Summary


a
0.

.5

.8

1.25

2.

^ U-6AI-4V h
Condition/Ht: BA
Form: 0.75 in. Plate
Specimen Type: CT
Orientation: LT
Frequency: 0.1 Hz
Environment: S.T.W.; RT

Yield Strength: 116.3 ksi


Ult. Strength: 125.7 ksi
Specimen Thk: 0.75 in.
Specimen Width: 5.008 in.
Ref: 88575
(1 of 1)

AK (MPaVin)
4

10

40

r ' i M'l'i

AK (MPaVin)
4

100

i ' i 'I'i'i

Stress Ratio: 0.5

40
100
i I i 11 IM

~1

10

-2

10
10

-3 10

10

ID"3

~~"

1"2

io~

~~~
_

ecu

-5

10

10

C=II I I I'M

10

JP
o
o 10
c

__

o 10

10-I

-a

_x"a
10

CD

10

10

10

TJ

10

10
"

10

10
-7

10

10

10

10
10.-8

1 , 1,1,1,

" 1 , 1,1,1,
4

10

40

10

I ,I lI,IlI ill
4

100

AK (KsiVin)

AK (KsiVin)
da/dN (I0_6in/cycle)

AK (KsiVin)

RMS %
Error

.5

.8

1.25

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


i

I I I I Hi
40
100

10

RMS %
Error

Life Prediction Ratio Summary

i-'

0.

2.

Figure 6.16.3.1.44
6-291

.5

.8

1.25

2.

\ Ti-6AI-4V hCondition/Ht: BA
Form: 0.63 in. Plate
Specimen Type: CT
Orientation: TL
Stress Ratio: 0.1
Frequency: 10 Hz

Yield Strength: 124.5 ksi


Ult. Strength: 136.4 ksi
Specimen Thk: 0.66 in.
Specimen Width: 2.55 - 2.554 in.
Ref: 90981
(1 of 3)

AK (MPaVin)
4

- I

10

i I 'I'l'l

40

100

' I M'l'l

(2 of 3)

AK (MPaVin)

-1

10

40

100

40

100

1 I I UMI

10

Environment: Dry Air; R.T.


10

10

:
10
2
io"

o 10

io

10

-D
"O

10

_e I
10
10

10

10
10

" 1 , 1,1,1,
4

1 , 1,1,1,

10

40

100

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)

10

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)

0.294
0.464
0.787
2.69
6.31
13.6
24.6
34.1
42.0
52.4
103.
254.
499.

8.24 (min)
9.
10.
13.
16.
20.
25.
30.
35.
40.
50.
60.
68.19 (max)

RMS %
Error

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

i-'

2.

RMS %
Error
16.33

Figure 6.16.3.1.45
6-292

Life Prediction Ratio Summary


I-

.5

.8

1.25

2.

Ti-6AI-4V
Condition/Ht: BA
Form: 0.63 in. Plate
Specimen Type: CT
Orientation: TL
Stress Ratio: 0.1
Frequency: 10 Hz

Yield Strength: 124.5 ksi


Ult. Strength: 136.4 ksi
Specimen Thk: 0.66 in.
Specimen Width: 2.55 - 2.554 in.
Ref: 90981
(3 of 3)

AK (MPaVin)
1

4
10
pr-Ti i i 11

AK (MPaVin)
4

40
100
_I I 11 nil

Environment: S.T.W.; R.T.

10

prii i in
W

40

100

' I H'l'l
10

-=i 10

-2

10

10

10
10

10

a?
10

o
6-10-4

o
^10"4

"-I ,o- 1
Z 10

10

10
"O
10

_.
10

10
10

10

10
.-8

10

10
4

10

40

100

i i 111 n
4
10

da/dN (10"6in/cycle)

16.
20.
25.
30.
35.
40.
50.
60.
70.
80.
87.57 (max)

Life Prediction Ratio Summary

0.

100

da/dN (10"6in/cycle)

AK (KsiVin)

10.2
10.6
20.7
29.9
37.6
47.7
62.1
98.9
133.
164
205.
264.

15.85 (min)

RMS %
Error
9.22

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , M.I

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary

0.

2.

Figure 6.16.3.1.45 (Concluded)


6-293

.5

.8

1.25

i-'

2.

i1 Ti-6AI-4V hCondition/Ht: BA
Form: 0.63 in. Plate
Specimen Type: CT
Orientation: TL
Stress Ratio: 0.1
Frequency: 1 Hz

Yield Strength: 124.5 ksi


Ult. Strength: 136.4 ksi
Specimen Thk: 0.66 in.
Specimen Width: 2.55 - 2.554 in.
Ref: 90981
(1 of 2)

AK (MPaVin)
4
10
I I i I MM

40
100
1I M HIM

- Environment: 3.5s NaCI; R.T.

(2 of 2)

AK (MPaVin)
10

- I ' I Tl'l

10
10

10

40

100

I ' I Tl'l

Environment: S.T.W.; R.T.

_L

~zz 10

"~

10

-3
10

10

6^10-

10

o
o^10-4

T3

10

10

10

10

10

10

10
4

10

40

J*
m

RMS %
Error
15.95

z
I , I,I,I,

I , I,I,I,

40

.5

10

100

25.4
36.7
72.5
94.5
106.
115.

185.
502.
1052.

50.
60.
69.64 (max)

.8

10

da/dN (10"6in/cycle)

18.51 (min)
20.
25.
30.
35.
40.

Life Prediction Ratio Summary


a
0.

10

AK (KsiVin)

0.423
4.99
17.5
37.4
58.6
81.2
115.
165.
256.
396.

-3 EI

10

z 10
-

AK (KsiVin)

da/dN (10'6in/cycle)

10.21 (min)
13.
16.
20.
25.
30.
35.
40.
50.
57.34 (max)

100

io"2

AK (KsiVin)
AK (KsiVin)

mJBn

~~

1.25

RMS %
Error
16.82

Figure 6.16.3.1.46
6-294

Life Prediction Ratio Summary

0.

.5

.8

1.25

^ Ti6AI-4V h
Condition/Ht: BA
Form: 0.63 in. Plate
Specimen Type: CT
Orientation: TL
Stress Ratio: 0.1
Frequency: 0.1 Hz

Yield Strength: 124.5 ksi


Ult. Strength: 136.4 ksi
Specimen Thk: 0.66 in.
Specimen Width: 2.55 in.
Ref: 90981
(1 of 1)

AK (MPaVin)
4

10

40

Ii i i I mi

= I ' I'l'l'l

AK (MPaVin)
1

100

ZD

I- I

10

40

' I 'I'llI

100

' I 'I'l'l
10

10

- Environment: S.T.W.; R.T

10
10

10

31

31

6-10-4

-3 |

10
a

10

"I

-4X>
10

>
D

10
-5

10

10
10

10
4

10

40

'

da/dN (10"6in/cycle)

Life Prediction Ratio Summary


i

0.

da/dN (10"6 in/cycle)

AK (KsiVin)

0.550
0.581
1.31
2.73
6.43
16.2
36.1
72.9
136.
400.
987.
2127.

9.81 (min)
10.
13.
16.
20.
25.
30.
35.
40.
50.
60.
69.91 (max)

RMS %
Error
47.90

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i I i I Hi
40
100

i i i ii

100

.5

.8

1.25

RMS %
Error

2.

Figure 6.16.3.1.47
6-295

Life Prediction Ratio Summary


r-

-1

0.

.5

.8

1.25

I--

2.

^ TI-6AI-4V
Condition/Ht: BA
Form: 2.79 in. Plate
Specimen Type: CT
Orientation: SL
Stress Ratio: 0.1
Frequency: 1 Hz

Yield Strength: 116.3 ksi


Ult. Strength: 125.7 ksi
Specimen Thk: 1.002 in.
Specimen Width: 1.996 in.
Ref: 88575
(1 of 1)

AK (MPaVin)
4

- I

10

' I 'I'l'l

40
-II

AK (MPaVin)
4

100

I 11 ll'l

10

40

100

1I I I I'l'l

p=II I'l'l'

10

10

Environment: S.T.W.; R.T.

-2

-2

10

10

10

10
-3

10

10

JD

^io"4

_CL

-3 I

10

o^10-

-3 I

10

xi

J10 >
a

-6

10

HP

10
D
"O

io"2

-o

10

10

10

-5

10
10

10

-6

10

10
i i i HI

>

10

10

i I'"

40

100

Life Prediction Ratio Summary


0.

.5

.8

1.25

10

111

I I I III

40

100

AK (KsiVin)

da/dN (1CT6in/cycle)

AK (KsiVin)

'

I I llll

AK (KsiVin)

RMS %
Error

_.

10

10

da/dN (10-6in/cycle)

AK (KsiVin)

RMS %
Error

Life Prediction Ratio Summary


.5

2.

Figure 6.16.3.1.48
6-296

.8

1.25

2.

^ Ti-6AI-4V r
Condition/Ht: BA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: TL
Frequency: 0.1 Hz
Environment: DIST WATER; RT

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(1 of 2)

AK (MPaVin)
4

- I

10

40

i I M'l'l

Stress Ratio: 0.1

(2 of 2)

AK (MPaVin)
4

100

' I M'l'l

- I

10

i I M'l'l

40

100

' I Tl'l

-2

10

10

10

10

10

o
:
^10"4

o
o 10
c

Z 10

Z 10
-o
10

"O

T3

io"2

:
Q
_

,.-1

10

_* I
10

-
10

10

10

10

10

10

10
10

10

Stress Ratio: 0.5

10

"o

I , I,I,I,

~ I , Mill
4

10

40

10

da/dN (10"6in/cycle)

100

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


0.

40

15.4
26.2
46.0
68.0
123.
227.
244.

26.53 (min)
30.
35.
40.
50.
60.
63.96 (max)

RMS %
Error
5.25

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , Mil.

" I , I.IJ.

100

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


i

0.

2.

Figure 6.16.3.1.49
6-297

.5

.8

1.25

2.

^ TJ-6AI-4V r
Condition/Ht: BA
Form: 0.63 in. Plate
Specimen Type: PTSF (max stress specified)
Orientation: TS
Frequency: 10 Hz
Environment: 3.5se NACL; RT
(1 of 1)

AK (MPaVin)
10

40

- I ' I 'IT

AK (MPaVin)
4

100
i i mi

10

40

100

I III

Yield Strength: 124.5 ksi


Ult. Strength: 136.4 ksi
Specimen Thk: 0.672 in.
Specimen Width: 1.5 in.
Ref: 90981

I III I-

Stress Ratio: 0.1


-2

-2

10

10

10

10

10

2
10~

o
\

^10~

6^10-

10"

m
,

^^

-z.

Z. 10

10

t"
'\
u
x>

10

10

~"

10

10

10

10
10

10
4

10

40

100

da/dN (10"6in/cycle)

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.468
0.619
3.48
9.24
18.4
26.0
31.8
42.3

9.65 (min)
10.
13.
16.
20.
25.
30.
34.71 (max)

RMS %
Error
3.51

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , Ml

- I , I,I,I,

Life Prediction Ratio Summary


.5

.8

RMS %
Error

Life Prediction Ratio Summary


0.

1.25

Figure 6.16.3.1.50
6-298

.5

.8

1.25

This page intentionally left blank

6-299

-I TI-6AI-4V I
Condition/Ht: BA
Form: 1.3 in. Forging
Specimen Type: WOL
Orientation: L-T
Stress Ratio: 0.02
Frequency: 0.1 20 Hz

Yield Strength: 111 - 111.5 ksi


Ult. Strength: 122.5 - 127.5 ksi
Specimen Thk: 1.25 in.
Specimen Width: 5 in.
Ref: MA005
(1 of 3)

AK (MPaVin)
1

10
ii

' I 'I'l'l

, _ ,

40
100
i i i nil

10

I- I 'I 'I'l'l
10

Environment: Lab Air; R.T.

10

10

(2 of 3)

AK (MPaVin)

-2

|_

40
T

100

1 I I I Mil

Environment: JP-4 Jet Fuel;


R.T.

^d10

10

10

10

10

a;

-2 Tt

10"
o

o 10

-i

10

10

10

10

X)

XI

"\
O

10

o
x>

10

XI

XI

10

10

10

10

10

10

10

10

10

10
4

10

40

100

da/dN (10_6in/cycle)

AK (KsiVin)

50.
60.
70.
80.

90.
99.83 (max)

Life Prediction Ratio Summary


i

0.

.5

.8

40

AK (KsiVin)

100

da/dN (10"6in/cycle)
0.109
0.161
0.581
2.11
6.74
15.5
28.5
44.9
91.5
175.
341.
680.
1542.
5517.
7448.

12.23 (min)
13.
16.
20.
25.
30.
35.
40.
50.
60.
70.
80.
90.
100.
101.83 (max)

0.0857
0.285
0.828
2.55
7.46
16.8
31.4
51.2
105.
193.
356.
724.
1946.
7407.

10.25 (min)
13.
16.
20.
25.
30.
35.
40.

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
26.85

1.25

2.

RMS %
Error
25.48

Figure 6.16.3.1.51
6-300

Life Prediction Ratio Summary


r-

0.

.8

1.25

\ TJ-6AI-4V h
Condition/Ht: BA
Form: 1.3 in. Forging
Specimen Type: WOL
Orientation: LT
Stress Ratio: 0.02
Frequency: 0.1 - 20 Hz

Yield Strength: 111 - 111.5 ksi


Ult. Strength: 122.5 - 127.5 ksi
Specimen Thk: 1.25 in.
Specimen Width: 5 in.
Ref: MA005
(3 of 3)

AK (MPaVin)
4

10

40

AK (MPaVin)
1

100

I I I llll>l
I I I 'I'll!
Environment: S.S.W.; R.T.

-1
-= 10

- I

10

' I 'I'l'l

40

100

' I 'l'l'l

-2

10

10

-3

10

10

10"2
o

o 10
10

a>

o
o 10

10"

'I

-5

10

10

10

_ -

xi

i4 "n

10 \
u
D

-
10

10
10

10

<E

10

10

10

10

1 , 1,1,1,

" 1 , 1,1,1,
10

40

10

100

da/dN (10"6in/cycle)

AK (KsiVin)
16.
20.
25.
30.
35.
40.
50.
60.
70.
80.

90.

99.93 (max)

Life Prediction Ratio Summary


i

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.223
0.775
1.93
4.83
11.6
23.6
43.3
72.7
154.
238.
392.
1007.
3207.
6205.

10.06 (min)

13.

0.

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
25.94

2 -7T

10

10

10

10

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


i

0.

2.

Figure 6.16.3.1.51 (Concluded)


6-301

.5

.8

1.25

2.

1 T1-6AI-4V I
Condition/Ht: BA
Form: 1.3 in. Forging
Specimen Type: WOL
Orientation: TL
Stress Ratio: 0.02
Frequency: 0.1 20 Hz

Yield Strength: 110 - 110.5 ksi


Uit. Strength: 124.5 - 125 ksi
Specimen Thk: 1.25 in.
Specimen Width: 5 in.
Ref: MA005
(1 of 3)

AK (MPaVin)
4

10

40

100

i- I

10

' I M'l'l

"1i

40
100
I > |i|M

Environment: JP-4 Jet Fuel;


R.T.

10

Environment: Lab Air; R.T.

(2 of 3)

AK (MPaVin)

.
1

10

10
~

10

P
10

10

10'
U

10"2

-10-4

10

Z. 10

Z 10
X
c
\
o
~ -6
10

-Jio
>

XI

10

o
XI

o
X

10
10

10
10

10

10

10
10

- 1 , 1,1,1,
4

1 , 1,1,1,

10

40

10
4

100

AK (KsiVin)
da/dN (10_6in/cycle)

AK (KsiVin)
13.
16.
20.
25.
30.
35.
40.
50.
60.
70.

80.
90.
100.
104.34 (max)

RMS %
Error
22.36

0.

.5

.8

0.131
0.220
0.621
2.09
6.93
16.8
31.5
49.4
97.8
183.
373.
892.
2136.
3491.

99.96 (max)

1.25

100

da/dN (10"6in/cycle)

AK (KsiVin)
16.
20.
25.
30.
35.
40.
50.
60.
70.
80.
90.

Life Prediction Ratio Summary


i

40

11.53 (min)
13.

0.118
0.217
0.576
1.93
6.57
16.4
31.1
48.6
94.9
183.
384.
868.
2005.
3911.
4776.

10.97 (min)

10

AK (KsiVin)

2.

RMS %
Error
27.07

Figure 6.16.3.1.52
6-302

Life Prediction Ratio Summary


i

.5

.8

1.25

TI-6AI-4V h
Condition/Ht: BA
Form: 1.3 in. Forging
Specimen Type: WOL
Orientation: TL
Stress Ratio: 0.02
Frequency: 0.1 20 Hz

Yield Strength: 110 - 110.5 ksi


Ult. Strength: 124.5 - 125 ksi
Specimen Thk: 1.25 in.
Specimen Width: 5 in.
Ref: MA005
(3 of 3)

AK (MPaVin)
4

10

40

AK (MPaVin)
1

100

_ I 1 I Tn
1 1 1 !<n
Environment: S.S.W.; R.T.
10

-I
10
>

-3 EI

io"2

o
u 10

10" E

10

-5

10

Z 10

Jio
>

_K
,-s

10

10

10

10

10
10

10
.-6

- i , i,i,i,
4

10

i 1 i! 111
40

10

'

I ' 'III

100

da/dN (10"6in/cycle)

AK (KsiVin)

10

40

100

AK (KsiVin)

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

0.217
0.620
1.48
3.76
9.37
19.4
35.0
57.6
126.
229.
399.
781.
1823.
5139.
6727.

10.11 (min)
13.
16.
20.
25.
30.
35.
40.
50.
60.
70.
80.
90.
100.
102.34 (max)

RMS %
Error
33.82

xi

10

10

10

10

10

u
\

1 ' I Tl'l=1

10
J0)

100

10

-3

^10"
\
c
_

40

10

10
o

10

b I ' I Tl'l

3 _

Life Prediction Ratio Summary


.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


i

.5

2.

Figure 6.16.3.1.52 (Concluded)


6-303

p-

.8

1.25

^ Ti-6AI-4V I
Condition/Ht: BETA PROCESSED - MA
Form: 0.13 in. Sheet
Specimen Type: CT
Orientation: LT
Frequency: 10 Hz
Environment: DRY AIR; RT
(1 of 1)

AK (MPaVin)
4
1

10

40

I M'l'lI

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 91332
AK (MPaVin)
1

100

' I 'I'l'l

Stress Ratio: 0.1

4
_

10
I

40

100

I I

10
10

10

10

10
-3

10

10

.2
_0)

o
6^10-4

-3 |

10

2
10~ o
o
\

Z 10
"O

10

tz

10
T3
10

z
4.4 "n
\
u

'

"O

_ I
-5

10

-7

10

10

10

10
i

I I I I Hi

10

.-8

10

i i 1111

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


0.

40

100

da/dN (10-6in/cycle)

AK (KsiVin)

4.71
6.46
11.0
15.2
21.3
52.5
79.1

23.05 (min)
25.
30.
35.
40.
50.
59.48 (max)

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
4.21

'1

10

10

10

10"

.5

.8

1.25

RMS %
Error

2.

Figure 6.16.3.1.53
6-304

Life Prediction Ratio Summary


,

0.

.5

1-i

.8

1.25

2.

Ti-6AI-4V
Condition/Ht: BETA PROCESSED - MA
Form: 0.3 - 0.5 in. Plate
Specimen Type: CT
Orientation: LT
Frequency: 10 Hz
Environment: DRY AIR; RT

40

' I 'I'I'I

AK (MPaVin)
1

100

-1

' I 'I'I'I

10

Stress Ratio: 0.1

10

100

_<p

10"2 o

10

10

10

2
io"

J
f

10

_B I
10

10

o
\

6-10-4
-3 |

:
10

Jio \

:
_K

10
-5

10

10

:
10

10

-= 10

10
10

10

-3

ID"3

"O

40

-2

10

10

10

10
\
c

I III I-

- I

10

I III

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 91332

(1 of 1)

AK (MPaVin)

" I , KM,
4

I , I,I,I,

10

40

10

- i , ,u,
4

100

da/dN (10"6in/cycle)

Life Prediction Ratio Summary

100

da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error

Life Prediction Ratio Summary


i

0.

40

2.38
4.72
9.03
15.2
23.0
28.9
42.1
95.8
97.0

16.77 (min)
20.
25.
30.
35.
40.
50.
60.
60.18 (max)

RMS %
Error
15.26

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , I,!,I,

.5

.8

0.

1.25

Figure 6.16.3.1.54
6-305

.5

.8

1.25

2.

^ TI-6AI-4V r
Condition/Ht: BETA PROCESSED - MA
Form: 3 in. Plate
Specimen Type: WOL
Orientation: L-T
Frequency: 1 Hz
Environment: LAB AIR; RT
(1 of 2)

AK (MPaVin)
4

= I

10

Yield Strength: 130.4 ksi


Ult. Strength: 138.1 ksi
Specimen Thk: 1 in.
Specimen Width: 2.55 in.
Ref: UD008

' I 'I'l'l

40
100
-1i iililil

10

40

I
= I ' I 'I'l'l
Stress Ratio: 0.5

10

Stress Ratio: 0.1

(2 of 2)

AK (MPaVin)
100

' I 'I'l'l
10

10
10

10

a>
2
10

10

o 10

'I

-=ho-3E

10~

-^

-5

10

L~O

10

10 \
u

-u

10
10

10

10

10

10

10

'

LLL

i i 11 n

10

40

100

AK (KsiVin)

RMS %
Error
12.51

9.
10.
13.
16.
16.76 (max)

6.50
27.0
40.0

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

100

0.114
0.132
0.316
0.874
1.84
4.17
15.2
19.5

6.57 (min)
7.
8.

0.493
0.611
0.874
2.24

14.50 (min)
16.
20.
25.
30.
35.
38.26 (max)

40

da/dN (10-6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

10

AK (KsiVin)

2.

RMS %
Error
8.73

Figure 6.16.3.1.55
6-306

Life Prediction Ratio Summary


i-

0.

.5

.8

1.25

2.

^ Ti6Al - 4V r
Condition/Ht: DB
Form: 0.63 - 1.5 in. Plate
Specimen Type: CT
Orientation: T-L
Frequency: 6 Hz
Environment: DRY AIR; RT

Yield Strength: 115 - 153 ksi


Ult. Strength: 126 - 165 ksi
Specimen Thk: 1 in.
Specimen Width: 4.94 - 6 in.
Ref: 88579
(1 of 2)

AK (MPaVin)

-2

10

40

100

Stress Ratio: 0.3

-=

-=

10

10

J2
t
o
:
o^lO"4

10"3

:
10

-Z. 10

-ho
>

10
-

xi

X>

10

6^10-4

-A-o
10
D
D

10

10

10

10

10

10

1 , 1,1,1,

~ 1 , 1,1,1,
4

"*"

10

10

10

10

10

10

-6

(2 of 2)

AK (MPaVin)

4
10
40
100
- I i I >|'l'l
I ' I 'l'l'l
-1
Stress Ratio: 0.08
10

o
"

10

40

10

100

i , i,i,i,

i , i,1.1.

40

da/dN (10"6in/cycle)

1.59
5.14
12.5
21.5
36.3
50.5

.5

.8

1.25

14.9
21.1
34.7
57.3
157.
359.
1368.

13.23 (min)
16.
20.
25.
30.
35.
37.82 (max)

Life Prediction Ratio Summary


0.

da/dN (10"6in/cycle)

AK (KsiVin)

0.153
0.156
0.208
0.331

7.88 (min)
8.
9.
10.
13.
16.
20.
25.
30.
32.73 (max)

RMS %
Error
10.63

100

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

2.

RMS %
Error
8.89

Figure 6.16.3.1.56
6-307

Life Prediction Ratio Summary


a
i

0.

-i

.5

.8

1.25

2.

I TI-6AI-4V h
Condition/Ht: DB
Form: 8 in. Plate
Specimen Type: CT
Orientation: T-L
Frequency: 1 Hz
Environment: S.T.W.; RT

Yield Strength: 118 ksi


Ult. Strength: 128 ksi
Specimen Thk: 0.992 in.
Specimen Width: 6 in.
Ref: 85837
(1 of 1)

AK (MPaVin)
4

= i

40
100
1i I i I iMI
'i'i'ir

AK (MPaVin)
4

10

- Stress Ratio: 0.08

=q
10

10

40

100

I III I-

I III

10

10
-i

10

10

10

10

_0)

io"
o

u 10
-3 |

10

10
-6
10

-3

*~"
D
X)

-o

10

10

_K
10
-"~

10

10

10

10

10
.-8

10

10
4

10

40

100

I , hi,I,

I , I,I,I,

40

AK (KsiVin)

10

100

AK (KsiVin)

AK (KsiVin)

da/dN (10_6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)
0.296
0.442
1.81
7.90
25.4

12.21 (min)
13.

16.
20.
25.
30.
35.
40.
50.

44.8
62.2

86.3
226.
380.

54.03 (max)

RMS %
Error
16.59

10

10
o
"

.92
I
o
6^10-4
c

10

Life Prediction Ratio Summary


0.

.5 .8

RMS %
Error

Life Prediction Ratio Summary


0.

1.25
Figure 6.16.3.1.57
6-308

.5

.8

1.25

i-'

2.

TI-6AI-4V
Condition/Ht: DB
Form: 8 in. Plate
Specimen Type: CT
Orientation: S-T
Frequency: 1 Hz
Environment: S.T.W.; RT

Yield Strength: 114 ksi


Ult. Strength: 128 ksi
Specimen Thk: 0.993 in.
Specimen Width: 4.94 in.
Ref: 85837
(1 of 1)

AK (MPaVin)
4

- I

10

' I 'I'll

40

AK (MPaVin)
1

100

' 1 'l'l'l

Stress Ratio: 0.08

= I

10

40

' I M'l'l

100

' I 'I'l'l=

10

10

10

10

10

10

10

JE

io"

J
o
^10"4
c
_

-3 |

10

o
6^10-4

10

Z 10
a

10

o
-a

"o

10

XI

- 10 >
o

_fi

10

10

10

10

10

10

10
10

.-5

2 10"S
"O

1 ,1,1,1,

- 1 ,1,1,1,
4

10

40

10
4

100

da/dN (10"6in/cycle)

AK (KsiVin)

100

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


0.

40

0.390
0.718
4.61
11.0
19.9
31.3
48.3
81.1
151.
496.

9.39 (min)
10.
13.
16.
20.
25.
30.
35.
40.
47.88 (max)

RMS %
Error
11.31

10

AK (KsiVin)

AK (KsiVin)

.5

.8

1.25

RMS %
Error

2.

Figure 6.16.3.1.58
6-309

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

I Ti-6AI-4V I
Condition/Ht: DB + 2DBTC
Form: 8 in. Plate
Specimen Type: CT
Orientation: TL
Frequency: 1 Hz
Environment: S.T.W.; RT

Yield Strength: 114 ksi


Ult. Strength: 128 ksi
Specimen Thk: 0.996 in.
Specimen Width: 6 in.
Ref: 85837
(1 of 1)

AK (MPaVin)
4

10

40

AK (MPaVin)
1

100
1

- I 1 I 'l'l'l
i ' 1 'l'l'l
Stress Ratio: 0.08

- I

10

' I 'I'l'l

40

100

' I 'l'l'l

-2

-2

10

10

10

10

-3

10

10

fci o-+

o 10

/
_

10

-5

10"

10

10

o
\

-o

'1
N

'

-z.
^
in u

Z 10

Z 10

2 T:

<D

10

X)

10

X3

_I
10
10

10

10

10

10

10

10

- i ,

I,I,I,
4

i ,

10

I,I,I,
40

10
4

100

AK (KsiVin)
AK (KsiVin)

100

1.02
2.18
7.62
23.1
45.9
73.5
110.
249.
536.
601.

60.
62.46 (max)

Life Prediction Ratio Summary


0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (I0"6in/cycle)

13.92 (min)
16.
20.
25.
30.
35.
40.
50.

RMS %
Error
6.60

10

AK (KsiVin)

.5 .8

RMS %
Error

Life Prediction Ratio Summary


i

.5

1.25
Figure 6.16.3.1.59
6-310

.8

1.25

2.

T1-6AI-4V
Condition/Ht: DB + 2DBTC
Form: 8 in. Plate
Specimen Type: CT
Orientation: ST
Frequency: 6 Hz
Environment: DRY AIR; RT

Yield Strength: 114 ksi


Ult. Strength: 128 ksi
Specimen Thk: 0.983 in.
Specimen Width: 4.95 in.
Ref: 85837
(1 of 1)

AK (MPaVin)
4

10

40

AK (MPaVin)
4

100

- I
-2

10

' I 'l'l'l

10

io"

(J

6-10-4
10"3E

J
f

tz

_*
-6

10

z: 10
"O

-2.-0

10

_^"o
10

o
10

10

10

10
:

-7

10

10

10

10
10

10-3

.22
2

6^10"+
\
c
_

-o

100

-o

' I M'l'l

40

10

10

Z 10

10

10

- Stress Ratio: 0.08

- i .i.i.i,
4

i ,I,I,I,

10

40

10
4

100

da/dN (10_6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


0.

40

100

da/dN (10~6in/cycle)

AK (KsiVin)

2.46
5.88
7.97
29.9
32.1

14.18 (min)
16.
20.
25.
26.83 (max)

RMS %
Error
11.46

10

AK (KsiVin)

AK (KsiVin)

.5

.8

RMS %
Error

Life Prediction Ratio Summary


0.

1.25

Figure 6.16.3.1.60
6-311

.5

.8

1.25

I Ti-6AI-4V h
Condition/Ht: DB + 4DBTC
Form: 8 in. Plate
Specimen Type: CT
Orientation: TL
Frequency: 1 Hz
Environment: S.T.W.; RT

Yield Strength: 115 ksi


Ult. Strength: 126 ksi
Specimen Thk: 0.99 in.
Specimen Width: 6 in.
Ref: 85837
(1 of 1)

AK (MPaVin)
1

i- I

10

40
i

' I M'l'l

AK (MPaVin)
4

100

- I

I i I i|i|

10

' I M'l'l

40

100

' I M'l'l

Stress Ratio: 0.08

10

-2

-2

10

10

10
10

10
Q)

10

o
fri"4

-3 I

10

Z 10

10

10

10

10

10
-7

10

10

10
10

10
4

10

40

100

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)
13.

16.
20.
25.
30.
35.
40.
50.
54.46 (max)

Life Prediction Ratio Summary


i

0.

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.255
0.475
2.15
9.51
25.4
42.9
76.1
132.
171.
281.

11.85 (min)

RMS S
Error
11.49

10

AK (KsiVin)

.5

RMS %
Error

r~

.8

Life Prediction Ratio Summary


0.

1.25

Figure 6.16.3.1.61
6-312

.5

.8

1.25

H Ti-6AI-4^Jv
Condition/Ht: DB + TR
Form: 1.5 in. Plate
Specimen Type: CT
Orientation: S-T
Frequency: 1 Hz
Environment: S.T.W.; RT

Yield Strength: 111 ksi


Ult. Strength: 128 ksi
Specimen Thk: 1 in.
Specimen Width: 5 in.
Ref: 88579
(1

AK (MPaVin)
4

_ I

10

40

i I >|i|i|

1)

AK (MPaVin)

i | i|i|i|

100

-i

10

- Stress Ratio: 0.08

io"2

10

| i |i|,|

40
|

100

, ,|,,,|

10

10"2
-1

-1

10

IQ"3

io"3

<x>

1"
o

<D

-^

^10"4
\
c

-3|

-'
zio~5
a
\
o
"^-6
10

2 10-

>
x>

-6
10

o
\

10

io2

(D

\
-|
10 3 E

>

n/cyc

-i

"=

10

\
o
"

II

' p

10

sE

10

>

'

'

"D

-5

-5

10

10

io-7

io"7

-6

-6

10

10

^-8
1

m"9 -

I , LI,I,

"1,1 ,1,1.
10

40

100

I , I,I,I,

I , I,I,I,

40

da/dN (10"6in/cycle)

10.12 (min)
13.
16.
20.
25.
30.
35.
4-0.
44.78 (max)

RMS %
Error
11.17

0.166
0.420
2.06
9.96
26.8
51.5
89.6
150.
339.

0.

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


i

100

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


0.

2.

Figure 6.16.3.1.62
6-313

.5

.8

1.25

2.

i Ti-6AI-4V I
Condition/Ht: DBT + PC
Form: 2.5 in. Plate
Specimen Type: CT
Orientation: TL
Frequency: 1 Hz
Environment: S.T.W.; RT

Yield Strength: 122 ksi


Ult. Strength: 135 ksi
Specimen Thk: 0.35 in.
Specimen Width: 7.4 in.
Ref: 88579
(1 of 1)

AK (MPaVin)
4

- I

10

i I i|i|'|

40

AK (MPaVin)
4

100

' | U'l'l

- I

100

' I 'I'l'l

10

10

10

-3

10

10

io"2

~~

"

o
6-10-4

o^10-4

-3 I

-3 |

10

10

-5

10

10

XJ

XI

10

_K h10

"o

XI

_fi r10

o
x

10

10

'
10

III I

10

10

10

x>

' I M'l'l

40

10

- Stress Ratio: 0.08

_0J

10

10

10

I , I,I,I,

10
4

10

40

10
4

100

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


r~

0.

40

100

da/dN (I0"6in/cycle)

AK (KsiVin)

0.256
0.623
1.87
11.1
30.7
41.6

10.37 (min)
13.
16.
20.
25.
27.18 (max)

RMS %
Error
23.75

10

AK (KsiVin)

.5

-i

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


i

0.

2.

Figure 6.16.3.1.63
6-314

.5

.8

1.25

\ Ti-6AI-4V h
Condition/Ht: DBTC
Form: 0.62 - 0.63 in. Plate
Specimen Type: CT
Orientation: L-T
Frequency: 1 Hz
Environment: DRY AIR; RT

4
p=ii

10

40

Yield Strength: 138 - 140 ksi


Ult. Strength: 148 - 150 ksi
Specimen Thk: 0.496 - 0.5 in.
Specimen Width: 6 in.
Ref: 88579;85837
(1 of 2)

AK (MPaVin)

(2 of 2)

AK (MPaVin)
4

100

10

40

- I ' I 'I'M

| i | i|i|

100

I ' I Tl'l

_1

Stress Ratio: 0.3


10

~ 10

10

i_

-^

10

10

"f &

-J10 >

- -

"o

10

j5

[!

10

-7

10

zzz

10
4

10

40

I , l.l.l,

I , I,I,I,

40

100

da/dN (10"6in/cycle)

16.
20.
25.
30.
35.
40.
50.
58.30 (max)

RMS %
Error
10.40

.5

.8

1.25

0.513
0.602
3.74
9.00
18.7
43.7
115.
295.
663.
2273.
4415.

9.83 (min)
10.
13.
16.
20.
25.
30.
35.
40.
50.
56.14 (max)

Life Prediction Ratio Summary


0.

da/dN (10"6in/cycle)

AK (KsiVin)

3.92
8.55
16.7
28.3
51.6
98.9
191.
757.
1723.

13.74 (min)

100

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

10

RMS 95
Error
10.25

Figure 6.16.3.1.64
6-315

Life Prediction Ratio Summary

0.

.5

.8

1.25

I Ti-6AI-4V I
Condition/Ht: DBTC
Form: 1.25 - 1.5 in. Plate
Specimen Type: CT
Orientation: L-T
Frequency: 1 Hz
Environment: S.T.W.; RT

- I

Yield Strength: 117 - 125 ksi


Ult. Strength: 129 - 138 ksi
Specimen Thk: 0.99 - 1 in.
Specimen Width: 6 - 7.4 in.
Ref: 88579;85837
(1 of 2)

AK (MPaVin)
4
10
40 100
' I 'I'l'l
I ' I 'l'l'l

Stress Ratio: 0.08

- I I I 'I'l'l

"=

-3

10

~~~

2
io"

io

^~
_

Z 10
10

_K l
10
__

o
o 10

-s
10

*^

2
io'

~*

o
fcl 0"+

-o

_' I
10

"~"

10

10

10

10

10

10

10

-^
"=

10

10

10

~o

(2 of 2)

10
"

-o

I ' I 'I'l'l

Stress Ratio: 0.3

10

AK (MPaVin)
4
10
40 100

I , I,I,I,

~ I , I, I,I,
4

10

10

40

10

I ,

da/dN (10"6in/cycle)

0.

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.131
0.201
0.341

0.592
2.49
6.28
13.5
27.4
49.2

83.9
99.2

Life Prediction Ratio Summary


i

40

0.112

6.24 (min)
7.
8.
9.
10.
13.
16.
20.
25.
30.
35.
36.57 (max)

RMS %
Error
37.08

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

1 , 1,1,1,

,1,1
4

100

10

1~.i

.5 .8

'

1.25

2.

RMS %
Error

Life Prediction Ratio Summary


0.

Figure 6.16.3.1.65
6-316

.5

.8

1.25

Ti-6AI-4V r
Condition/Ht: DBTC
Form: 1.25 in. Plate
Specimen Type: CT
Orientation: L-T
Frequency: 1 Hz
Environment: DRY AIR; RT

Yield Strength: 125 ksi


Ult. Strength: 137 ksi
Specimen Thk: 1 in.
Specimen Width: 6 in.
Ref: 88579
(1 of 1)

AK (MPaVin)
4

10

AK (MPaVin)
1

40
100
I t 111111

4
10
r=-\i i i M't

40
100
1' i i Hi'i
10

10
10

10
u
6-10-4
c

-3 |

10

,-s

T3

10

-J10 >
-o

10
10

10
10

10
4

10

40

LL

I I I I III
4

100

da/dN (10'6in/cycle)

13.
16.
20.
25.
30.
35.
40.
50.
59.95 (max)

Life Prediction Ratio Summary

0.

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.296
1.39
4.45
12.8
27.3
43.3
67.5
111.
281.
782.

10.00 (min)

RMS %
Error
35.47

Li

I I 11II

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'

10

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


-r-

0.

2.

Figure 6.16.3.1.66
6-317

.5

.8

1.25

!-
2.

\ Ti-6AI-4V h
Condition/Ht: DBTC
Form: 1.25 - 1.5 in. Plate
Specimen Type: CT
Orientation: TL
Frequency: 1 Hz
Environment: DRY AIR; RT

Yield Strength: 119 - 128 ksi


Ult. Strength: 134 - 139 ksi
Specimen Thk: 0.96 1 in.
Specimen Width: 6 7.46 in.
Ref: 88579
(1 of 2)

AK (MPaVin)
1

10

40

(2 of 2)

AK (MPaVin)
4

100

10

40

- I I I 'I'H

F=ii I i Mill

100

I ' I 'l'l'l

10

Stress Ratio: 0.3

10
10

-3

10

u
o
\

10

10~

^io"4
c

Z 10

"o
\
o
O

10

-6

'I

^^
ZL

tz

m~ ^
u
TJ

-5

10

'

10
10

10
4

10

40

"

I , I,I,I,

I , l,l,l,

40

100

da/dN (10"6in/cycle)

RMS %
Error
8.42

.5

.8

1.25

0.458
0.489
1.56
4.42
12.3
25.7
41.8
68.0
113.
276.
694.

9.82 (min)
10.
13.
16.
20.
25.
30.
35.
40.
50.
56.48 (max)

Life Prediction Ratio Summary


a
i

da/dN (10~6in/cycle)

AK (KsiVin)

0.842
1.22
3.71
7.71
14.1
25.2
43.4
71.4
162.
334.

12.36 (min)
13.
16.
20.
25.
30.
35.
40.
50.
57.13 (max)

100

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

2.

RMS %
Error
18.51

Figure 6.16.3.1.67
6-318

Life Prediction Ratio Summary


a
i

0.

.5 .8

1.25

2..

TJ-6AI-4V
Condition/Ht: DBTC
Form: 1.5 - 2.5 in. Plate
Specimen Type: CT
Orientation: TL
Stress Ratio: 0.08
Frequency: 1 Hz

Yield Strength: 119 - 125 ksi


Ult. Strength: 132 - 135 ksi
Specimen Thk: 0.962 - 1 in.
Specimen Width: 4.94 - 7.4 in.
Ref: 85837;88579
(1 of 2)

AK (MPaVin)
4

10

40
-ii

' I M'l'l

100

10

10

40

100

da/dN (10"6in/cycle)

1 ' I 'I'l'l

10

40

10

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.449
0.449
0.891
2.19

9.95 (min)
10.
13.
16.
20.
25.
30.
32.61 (max)

0.421

0.455
0.866
1.41
2.06

2.81
5.66
9.65
17.9

4.92
13.9

25.9
35.8

36.8
71.3

Life Prediction Ratio Summary


a o
0.

100

AK (KsiVin)

5.90 (min)
6.
7.
8.
9.
10.
13.
16.
20.
25.
29.65 (max)

RMS S
Error
>100.0

40

- Environment: S.T.W. & JP-4;


_
R.T.

AK (KsiVin)
AK (KsiVin)

10

-Ml 'I'l'l

i i i i|i|

Environment: S.T.W.; R.T

(2 of 2)

AK (MPaVin)

.5

.8

1.25

2.

RMS %
Error
7.49

Figure 6.16.3.1.68
6-319

Life Prediction Ratio Summary


0.

.5

.8

1.25

i Ti-6AI-4V
Condition/Ht: DBTC(RA)
Form: 0.63 in. Plate
Specimen Type: CT
Orientation: LT
Frequency: 1 Hz
Environment: DRY AIR; RT

Yield Strength: 134 ksi


Ult. Strength: 145 ksi
Specimen Thk: 0.5 in.
Specimen Width: 6 in.
Ref: 88579
(1 of 1)

AK (MPaVin)
4

10

40

1i I i I'l'l

' I 'I'l'l

AK (MPaVin)
4

100

= I

ni

10

' I 'I'l'l

40

100

' I 'I'l'l

10

Stress Ratio: 0.3

10

-2

10

10

10

10
-3

10

10

_0)

io"2

o
\

o 10
10

c^o'4
10

E
Z 10

10
o
~

10

10

D
T3

-6

"a

10

-R
-6

10

10

10

10

10

10

10
' i 'iHI

10

'

10

10

i i i iii

40

100

35.
40.

40.98 (max)

Life Prediction Ratio Summary

0.

100

55.5
116.
196.
194.

30.88 (min)

40

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
13.38

.5

.8

1.25

RMS %
Error

2.

Figure 6.16.3.1.69
6-320

Life Prediction Ratio Summary


i

.5

.8

1.25

H T1-6AI-4V r
Condition/Ht: HIP 1650F 15 KSI
Form: Casting
Specimen Type: CT
Orientation:
Frequency: 0.1 20 Hz
Environment: LAB AIR; RT
(1 of 1)

AK (MPaVin)
4

10

Yield Strength: 60 ksi


Ult. Strength:
Specimen Thk: 0.1 in.
Specimen Width: 0.999
Ref: WL011

1 in.

AK (MPaVin)
4
10
pr-Ti i i FT
MM

40
100
i I i I mi

40

100

' I 'I'll
10

10
10

10
O

o 10
_J

c
"O

-o

_
10

10

-5

_ -

10

10
10
10
10
4

10

40

100

da/dN (10"6in/cycle)

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.158
0.529

1.51
5.23
15.3
25.5
55.0
78.0

Life Prediction Ratio Summary


i

0.

40

0.0490
0.0597
0.0993

7.64 (min)
8.
9.
10.
13.
16.
20.
25.
30.
35.
36.32 (max)

RMS %
Error
17.83

Li

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

11in
10

.5

.8

RMS %
Error

Life Prediction Ratio Summary


i

0.

1.25

Figure 6.16.3.1.70
6-321

.5

.8

1.25

2.

i TJ-6AI-4V h
Condition/Ht: MA
Form: 0.1 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: L-T
Frequency: 1 6 Hz
Environment: DRY AIR; RT
(1 of 3)

AK (MPaVin)
4

10

= I ' I 'I'l'l
10

40

I ' I 'ITI

10

_ 10
""

Stress Ratio: 0.3

-1

-A
10

io"2

T&

10

_0
o

10

10

o
10

-z. io

"O

-5

10

10

40

10

10

"

- 1 , 1,1,1,
4

100

da/dN (I0"6in/cycle)

RMS %
Error
11.20

9.
10.
13.
16.
17.28 (max)

HD
i-'

.5

.8

100

1.25

0.523
0.511
0.777
1.43
2.27
5.06
7.46
10.1

6.62 (min)
7.
8.

Life Prediction Ratio Summary


0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.691
0.785
1.15
1.67
4.27
7.80
13.5
22.3
37.8
41.9

7.65 (min)
8.
9.
10.
13.
16.
20.
25.
30.
30.60 (max)

1 , 1,1,1,

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

_*
-6
10

10

I , I,I,I,

_*;o

10

10

I , I ,l,l,

10

io"2

^10"4

10

-1

10

10

10

100

10

40

I ' I 'I'l'l

10

^io"4

10

- I I I 'I'l'l

_L

Stress Ratio: 0.08

(2 of 3)

AK (MPaVin)

100

10

Yield Strength: 137 ksi


Ult. Strength: 147 ksi
Specimen Thk: 0.092 - 0.101 in.
Specimen Width: 23.98 - 24.22 in
Ref: 86575

2.

RMS %
Error
13.10

Figure 6.16.3.1.71
6-322

Life Prediction Ratio Summary


0.

.5

.8

1.25

2.

1 Ti-6AI-4V r
Condition/Ht: MA
Form: 0.1 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: LT
Frequency: 1 6 Hz
Environment: DRY AIR; RT

= I

10

' I 'I'l'l

40

I1

Yield Strength: 137 ksi


Ult. Strength: 147 ksi
Specimen Thk: 0.092 - 0.101 in.
Specimen Width: 23.98 - 24.22 in
Ref: 86575

(3 of 3)

AK (MPaVin)

AK (MPaVin)
1

100

' I U'l'l

Stress Ratio: 0.5

4
T=\

10

I I Mill

40
1

100

I I |l|l|

10

10
10

10

10

10
-3

10

10

o
\

o 10

-3 IE

-no"2
o

o
10

-3l

10

10
-5

10

10

10
"O

T3

10

10

10
-5

10

10
-7

10

10

10

10
i

LU

111in

'

10

10

111HI

40

'

10

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

I I I I III
40
100

I I 11II

100

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

0.930
1.53
2.30
5.34
9.87
21.1
22.4-

8.06 (min)
9.
10.
13.
16.
20.
20.31 (max)

RMS %
Error
3.74

XI

10

Life Prediction Ratio Summary


i

r-

.5 .8

1.25

RMS %
Error

Life Prediction Ratio Summary


i

0.

2.

Figure 6.16.3.1.71 (Concluded)


6-323

.5

.8

1.25

^ TJ-6AI-4V I
Condition/Ht: MA
Form: 0.1 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: LT
Stress Ratio: 0.08
Frequency: 1 6 Hz
(1 of 2)

AK (MPaVin)
4

10

-Ml 'I'll
-2

10

10
O
4

40

o
"O

10
~3

10

-zz

-zz

10

10

jj

1 , 1,1,1,

" 1 , 1,1,1,

40

10

-:: 10

10

a)

10

-zz 10"

10
"O

.8

i"

'\
u
x>

-= 10

-7

-zz 10

10

10

1 , 1,1,1,

- i , 1,1,1,
4

10

40

100

AK (KsiVin)

1.25

da/dN (10"6in/cycle)

AK (KsiVin)

0.447
0.504
0.747
1.16
1.90
3.24
15.0
28.2
37.2

5.67 (min)
6.
7.
8.
9.
10.
13.
16.
19.01 (max)

1.02
1.30
1.56
2.68
5.80
13.9
22.7
33.0
35.9

o
\

10

da/dN (10"6in/cycle)

.5

>
/

10

z:

_fi

10

10*

1f

-5

Z 10
X>

<D

~"

Life Prediction Ratio Summary


0.

Environment: S.T.W.; R.T.

100

8.05 (min)
9.
10.
13.
16.
20.
25.
30.
30.58 (max)

RMS %
Error
19.82

100

' I 'I'l'l

10

AK (KsiVin)
AK (KsiVin)

40

10

10

- I ' I 'I'l'l

j.

Environment: JP--4 Jet Fuel;


_ R.T.

-6

10

' 1 'I'l'l

(2 of 2)

AK (MPaVin)

100

6-10-

10

Yield Strength: 137 ksi


Ult. Strength: 147 ksi
Specimen Thk: 0.096 in.
Specimen Width: 24 in.
Ref: 86575

RMS %
Error
6.84

Figure 6.16.3.1.72
6-324

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

-\ Ti-6AI-4V r
Condition/Ht: MA
Form: 0.1 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: TL
Stress Ratio: 0.08
Frequency: 6 Hz
(1 of 2)

AK (MPaVin)
4

- I

__
10

10

' I 'I'l'l

_i

u^10-4

t= I

-7

10

10

io"

^NO"2

_0J

u
o 10

-&-

-3 |

- 10" E

10

T5

10

10

10
10

.10

i , i,i,i,

I , I,I,I,

40

10

10

10

' i ill
i i in

100

'

10

i i LLL
11 ii

40

100

AK (KsiVin)

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)

-a

10
=

-J10 >

da/dN (10"6in/cycle)

AK (KsiVin)

2.30
2.97
5.14
9.53
16.5
26.7
43.2
68.3
101.

11.52 (min)
13.
16.
20.
25.
30.

35.
40.
44.86 (max)

RMS %
Error
0.89

-d 10

10
2

' I 'I'l'l

10

_,

.-6

10

' I 'I'l'lI

100

"O

40

10

10
-z. 10

10

Environment: S.T.W.; R.T.

Environment: Dry Air; R.T.

(2 of 2)

AK (MPaVin)
4

40
100
r- I 'I'l'l

10

Yield Strength: 143 ksi


Ult. Strength: 151 ksi
Specimen Thk: 0.096 - 0.097 in.
Specimen Width: 24 in.
Ref: 86575

Life Prediction Ratio Summary


a
r

0.

.5

.8

1.25

2.

RMS x
Error

Life Prediction Ratio Summary


0.

Figure 6.16.3.1.73
6-325

.5

.8

1.25

\ Ti-6AI-4V I
Condition/Ht: MA
Form: 0.75 in. Plate
Specimen Type: CT
Orientation: LT
Frequency: 20 Hz
Environment: LAB AIR; RT

Yield Strength: 135.3 ksi


Ult. Strength: 137.6 ksi
Specimen Thk: 0.25 in.
Specimen Width: 2.5 in.
Ref: 88468
(1 of 2)

AK (MPaVin)
4

10

40

100

10

40

i- I ' I TIM
-= 10

Stress Ratio: 0.05

(2 of 2)

AK (MPaVin)
100

' I TIM
10

Stress Ratio: 0.3

-2

10

10

-1

10

-3

10

10
_QJ

-J10"2 P
o

_03

o 10

6-10-4

-3 |

f
4

Z 10
o

_E

10

10

10

10

icT \
o
10

10

10

10

i ,

- i , i,i,I,
4

10

10

,I,I,
40

10

da/dN (10-6in/cycle)

38.24 (max)

0.

.5

.8

100

0.342
0.429
0.995

8.78 (min)
9.
10.
13.
14.23 (max)

Life Prediction Ratio Summary


\

40

da/dN (10'6in/cycle)

AK (KsiVin)

0.171
0.716
2.86
6.34
10.0
14.9
25.1
38.4

16.
20.
25.
30.
35.

10

AK (KsiVin)

11.31 (min)
13.

RMS %
Error
29.60

' i iiHI

i i 11 ti

100

AK (KsiVin)
AK (KsiVin)

XI

10
10

Z 10

""

10

1.25

2.

RMS %
Error
26.53

Figure 6.16.3.1.74
6-326

3.46
4.08

Life Prediction Ratio Summary

0.

.5

.8

1.25

2.

TI-6AI-4V h
Condition/Ht: MA
Form: 0.63 in. Plate
Specimen Type: CT
Orientation: LT
Stress Ratio: 0.3
Frequency: 1 Hz

Yield Strength: 138 ksi


Ult. Strength: 148 ksi
Specimen Thk: 0.49 - 0.5 in.
Specimen Width: 6 in.
Ref: 88579
(1 of 2)

AK (MPaVin)
1

10

' I M'l'l

40

100

' I M'l'l

Environment: Dry Air; R.T.

(2 of 2)

AK (MPaVin)
4

= I
10

10

40

' I 'I'l'l

100

' I M'l'l

Environment: Lab Air; R.T.

10

10
10

10
10

0)

10

o
\

o^io-4

-3 |

10

_
10

10

o
x>

-5

Jio >
XI

10

-6

10

10

10
-7

10

10

10
'

10
1

10

40

100

da/dN (10"6in/cycle)

RMS %
Error
10.90

.5

.8

100

1.25

28.0
30.9
55.0
75.3
290.

10.36 (min)
13.
16.
20.
23.71 (max)

Life Prediction Ratio Summary


0.

I 1 HII

40

da/dN (10"6in/cycle)

AK (KsiVin)

4.75
8.13
21.1
69.4
504.
1996.
4131.

11.30 (min)
13.
16.
20.
25.
30.
33.26 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'

I ' I III

RMS %
Error
14.05

Figure 6.16.3.1.75
6-327

Life Prediction Ratio Summary


a
T-

0.

.5

.8

1.25

TI-6AI-4V hCondition/Ht: MA
Form: 1.25 in. Plate
Specimen Type: CT
Orientation: LT
Stress Ratio: 0.3
Frequency: 1 Hz

Yield Strength: 120 ksi


Ult. Strength: 134 ksi
Specimen Thk: 0.99 - 0.997 in.
Specimen Width: 6 - 6.01 in.
Ref: 85837
(1 of 2)

AK (MPaVin)
4

(2 of 2)

AK (MPaVin)

10

40
100
ni i i MIIIm
10
Environment: Dry Air; R.T.

- I

F=-1i I i Mil

-2

4
10
I I '{in

40
100
1 1 llll>l
-I

Environment: S.T.W.; R.T.

10

10

10

10

10

10
-3

10

10

_0J

-3 p.
10 E

-2 Tl

^10"

-3 I

10

10
10

o
-6

10

10

10

o
x>

10

10
10

-7

10

i i i i in
40
100

' i i i in
4
10

10

II 1 1

10

10

1 , 1,1,1,

10

da/dN (10"6in/cycle)

AK (KsiVin)
13.
16.
20.
25.
30.
32.09 (max)

.5

.8

100

1.25

0.388
0.443
0.629
2.75
10.7
34.2

8.19 (min)
9.
10.
13.
16.
20.
25.
30.
32.78 (max)

Life Prediction Ratio Summary


i

40

da/dN (10"6in/cycle)

AK (KsiVin)

1.00
2.76
10.4
21.6
40.9
47.5
53.8

11.70 (min)

0.

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
5.42

2.

RMS %
Error
20.41

Figure 6.16.3.1.76
6-328

57.1
74.2
92.0

Life Prediction Ratio Summary


o
0.

.5

.8

1.25

T1-6AI-4V h
Condition/Ht: MA
Form: 0.63 - 1.5 in. Plate
Specimen Type: CT
Orientation: L-T
Stress Ratio: 0.3
Environment: DRY AIR; RT

- I

10

' I 'I'l'l

Yield Strength: 120 - 138 ksi


Ult. Strength: 134 - 148 ksi
Specimen Thk: 0.67 1 in.
Specimen Width: 6 in.
Ref: 88579:84361 ;85837
(1 of 2)

AK (MPaVin)

(2 of 2)

AK (MPaVin)
1

40
100
-1I I I I mi

4
10
prIi | i |i|i|

40

100

40

100

10

Frequency: 1. Hz

10
10

10
O

l 0"+
10

10

-o

_. 10

T3

10

10
10

10

'

' 1111 n

10

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error
7.17

313.
679.
1469.

Life Prediction Ratio Summary


-r-

0.

.5

.8

AK (KsiVin)
6.36 (min)
7.
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
50.
58.57 (max)

144.

26.05 (min)
30.
35.
39.74 (max)

10

AK (KsiVin)

AK (KsiVin)

1.25

RMS %
Error
26.46

Figure 6.16.3.1.77
6-329

da/dN (10"6in/cycle)
0.131
0.139
0.183
0.272
0.426
1.67
5.32
16.1
34.5
49.6
68.8
108.
361.
747.

Life Prediction Ratio Summary


o
!-
1
r- T
2.
.5 .8 1.25
0.

I -R-6AI-4V r
EF Condition/Ht: MA
Yield Strength:
Ult. Strength:
Specimen Thk: 1 in.
Specimen Width: 2.55 in.
Ref: 88144

Form: 1 in. Plate


Specimen Type: CT
Orientation: TL
Stress Ratio: 0.1

AK (MPaVin)
4
10
40
100

- [

' I M'l'l

' I ' l'l'l

Environment: Lab Air; -65T;


_ Frequency: 0.1 Hz

(1 of 4)

AK (MPaVin)
4
10
40
100

- I ' I'l'l'l

10

' I M'l'l

Environment: Lab Air; -65T;


_ Frequency: 10. Hz

"~

10

&

10

-3 10

-3

10

10
"~~

2 u

_Q3

10"

,o-i

CD

6-10-4
c
_

10

z: 10

Z10
""~

10

10'\
o
-o

"*"""

-= 10

XI

10

10
10

10

II I I

10

10

10

o
10
\
c

(2 of 4)

I , LI,I,

.-8

10

10
40
AK (KsiVin)

10

0.

.5 .8

1.25

I , I,I,I,
4

Life Prediction Ratio Summary


i

"

100

RMS %
Error

0.

Figure 6.16.3.1.78
6-330

, I , l,l,
100

da/dN (10"6in/cycle)

Life Prediction Ratio Summary

2.

10
40
AK (KsiVin)

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error

10

10

.5

.8

1.25

Ti-6AI-4V f
Condition/Ht: MA
Form: 1 in. Plate
Specimen Type: CT
Orientation: TL
Stress Ratio: 0.1

Yield Strength:
Ult. Strength:
Specimen Thk: 1 in.
Specimen Width: 2.55 in.
Ref: 88144
(3 of 4)

AK (MPaVin)
1

10

-IM Tl'l
-2

EF

40

100

TI I i IM'!

Environment: Lab Air; 175F;


_ Frequency: 0.1 Hz

~=j

(4 of 4)

AK (MPaVin)

10

4
10
40
100
c=li i i Mill
r
I ' I Tl'l
Environment: Lab Air; 175T; 10
_ Frequency: 10. Hz

10

10

10
10

10

u 10
10

I?

-5

10

10

Jio >

o
10

10
10

10

10
10
-8

10

10

I I I I III

'I'll

10

40

100

AK (KsiVin)

10

40

da/dN (10"6in/cycle)

da/dN (I0"6in/cycle)

AK (KsiVin)

8.94
11.7
20.0
33.9
52.4
66.7
134.

17.93 (min)
20.
25.
30.

35.
40.
50.

197.

55.07 (max)

RMS %
Error

Life Prediction Ratio Summary


.8

100

AK (KsiVin)

AK (KsiVin)

1.25

RMS X
Error
11.38

Life Prediction Ratio Summary


0.

Figure 6.16.3.1.78 (Concluded)


6-331

-I-

T"

.5

.8

1.25

^ Ti-6AI-4V
Condition/Ht: MA
Form: 1 in. Plate
Specimen Type: CCP (max load specified)
Orientation: L-T
Frequency: 10 Hz
Environment: LAB AIR; RT
(1 of 2)

AK (MPaVin)
4

10

= I ' i 'I'l'l

Yield Strength: 132.5 ksi


Ult. Strength: 138 ksi
Specimen Thk: 0.25 in.
Specimen Width: 4 in.
Ref: MA006

40

100

I ' I 'l'l'l

Stress Ratio: -1.0

(2 of 2)

AK (MPaVin)
4
10
40 100

10

Stress Ratio: 0.5

-2

10

10

10

10

10

_2>
o

10

~
_

Z 10
"o

tz

"o

10

10

Jio
>

Jio
>

or

10

Ai

-5

10

10

10

10

-6

1
-= 10

10
10

Z 10

.-6

10

o^10-+
\
c
_

6^10"

io" ^

_gj
u

<~

_0J
2

I , I ,l,i,

~ I , I,I,I,
4

10

40

10

100

da/dN (lO^in/cycle)

RMS %
Error
9.11

Life Prediction Ratio Summary


,

0.

.5

.8

1.25

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.359
0.727
1.82
3.50
5.74
8.51
20.4
41.3
97.2
208.
300.
379.
552.
1771.

5.43 (min)
6.
7.
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
49.27 (max)

0.640
0.695
1.14
3.25
6.53
12.9
25.1
44.4
75.1
124.
323.
767.
1356.
1789.
2992.
3717.

8.85 (min)
9.
10.
13.
16.
20.
25.
30.
35.
40.
50.
60.
70.
80.
90.
92.48 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , I,I,I,

" I , I,I,I,

2.

RMS %
Error
18.52

Figure 6.16.3.1.79
6-332

Life Prediction Ratio Summary


r-

r-

0.

.5

.8

1.25

\ TJ-6AI-4V h
Condition/Ht: MA
Form: 0.38 in. Plate
Specimen Type: CCP (max load specified)
Orientation: LT
Stress Ratio: 0.02
Environment: LAB AIR; RT

10

(2 of 2)

AK (MPaVin)
1

40
100
I I I MI'I

- I ' I 'IT

Yield Strength: 137 ksi


Uli Strength: 145 ksi
Specimen Thk: 0.241 - 0.242 in.
Specimen Width: 3.952 - 3.953 in
Ref: MA002

(1 of 2)

AK (MPaVin)

10

40

i- i ' i 'H|'|

100

' I TIM

Frequency: 20. Hz

10

40

100

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error

12.01

0.

.5

.8

100

1.25

da/dN (10"6in/cycle)

AK (KsiVin)

0.0149
0.0198
0.0494

5.
6.
7.
8.

0.0759
0.113
0.198
0.404
2.48
5.73
15.8
18.2

9.
10.
13.
16.
20.
20.57 (max)

Life Prediction Ratio Summary


i

40

4.82 (min)

0.0805
0.0750
0.0933
0.161
0.317
2.08
5.96
10.8
24.1
62.8
144.
322.

6.63 (min)
7.
8.
9.
10.
13.
16.
20.
25.
30.
35.
38.83 (max)

10

AK (KsiVin)

!-

2.

RMS 55
Error
9.55

Figure 6.16.3.1.80
6-333

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

Ti-6AI-4V r
Condition/Ht: MA
Form: 1.5 in. Plate
Specimen Type: CCP (max load specified)
Orientation: L-T
Stress Ratio: 0.02
Environment: LAB AIR; RT
(1 of 2)

AK (MPaVin)
1

10

b I ' I 'I'l'l

40

Yield Strength: 133 ksi


Ult. Strength: 142 ksi
Specimen Thk: 0.188 - 0.191 in.
Specimen Width: 3.957 - 3.964 in
Ref: MA002

1 ' I TIM

100

Frequency: 27. Hz

(2 of 2)

AK (MPaVin)
10

40
r

i ' i M'l'i

10

100
TTTTl

r~

10

Frequency: 30. Hz

-2

10

10

10

10
-3

10

10

o
o 10

0^10"*

-3 |

-3 |

10

10

10

10
10

o
XJ

"O

10

10
-5

10

10
10

10

10

10
.-8

10

10

10

40

100

0.113
0.450
3.03
8.73

Life Prediction Ratio Summary


I

0.

.5

.8

100

1.25

0.0829
0.0833
0.102
0.145

7.47 (min)
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
44.29 (max)

0.0306
0.0325
0.0509
0.0658
0.0835

5.91 (min)
6.
7.
8.
9.
10.
13.
16.
17.49 (max)

40

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (10-6in/cycle)

AK (KsiVin)

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
14.69

10

i-

2.

RMS %
Error
18.82

Figure 6.16.3.1.81
6-334

0.563
1.98
6.77
18.4

35.8
68.5
148.
306.

Life Prediction Ratio Summary


r-

0.

.5

.8

1.25

2.

H T-6AI--4V rr-n
Lh
Condition/Ht: MA
Form: 0.75 in. Plate
Specimen Type: CCP (max load specified)
Orientation: LT
Stress Ratio: 0.04

AK (MPaVin)
1

10

- I ' I 'I'l'l

40

of 1)

AK (MPaVin)
1

100

I ' I M'l'l

Environment: Lab Air; R.T.;


_ Frequency: 20. Hz

-"

10

10"2

4
_

10

. | - jT|

40
|

100

1 | .|.,.,

_L

10

-2

10
-i

10

io"3 ~

<a
2

1"
o

JD

l0"
\

V-'
5

2 10"

-3|
10 E

-z.

10 \
o

XI

-6

10

io-3

"

Yield Strength: 135.3 ksi


Ult. Strength: 137.6 ksi
Specimen Thk: 0.29 in.
Specimen Width: 6.011 in.
Ref: 88468

a>

io"2

03

o
\
-3|
10 NE
-'

o
o 10
^-^
Z10"5
-a
\
o

-z.
__ 10 \
o
T>

"4-
10

10

-5

-5

10

~ 10
-

io"7

io"7
-6

-6

10

10

I I.U

~ I , I . I,l,

m-8

10

40

irf8

" 1 , 1,1,1,
1

100

AK (KsiVin)
31.29 (min)
35.
4-0.
50.
59.30 (max)

RMS %
Error
7.38

40

100

da/dN (I0"6in/cycle)

AK (KsiVin)

18.7
24.3
41.3
93.2
220.

Life Prediction Ratio Summary


a
0.

10

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

I , I,I,I,

.5

.8

1.25

2.

RMS %
Error

Life Prediction Ratio Summary


0.

Figure 6.16.3.1.82
6-335

.5

.8

1.25

2.

H Ti-6AI-4V
Condition/Ht: MA
Form: Extrusion
Specimen Type: CT
Orientation: LT
Frequency: 6 Hz
Environment: DRY AIR; RT

Yield Strength: 123.5 ksi


Ult. Strength: 135.5 ksi
Specimen Thk: 0.993 - 0.995 in.
Specimen Width: 3.77 in.
Ref: 85837
(1 of 3)

AK (MPaVin)
4

- I

10

' I M'l'l

40

100

' I M'l'l

Stress Ratio: 0.08

(2 of 3)

AK (MPaVin)

-2

4
. |

10
T|i|

40
100
. | i|i|i|
a

Stress Ratio: 0.3

10

10

10

10

10
:

10

10

io'
O

o 10

fci o"
c

Q)

"""*

10

f
f

/
10

10

10

"a

10
""

_c h10

10
-7

-7

2
10" o
o
\

10"

z:
i "o
10 \
u
-u
10

10

10

10

10
10

" I , I,LI,
4

I , M,l

10

40

10

i ,

100

da/dN (10"6in/cycle)

RMS 56
Error
13.66

.5

T~

.8

100

1.25

0.973
3.65

11.48 (min)
13.
16.
20.

1.51
5.47
12.0
20.6
34.7
58.3

8.87
16.4

41.2

25.
30.

59.0

68.4

32.86 (max)

Life Prediction Ratio Summary


0.

,I.I,

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.496

11.52 (min)
13.
16.
20.
25.
30.
34.01 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i , i

.Mi
4

RMS %
Error
14.94

Figure 6.16.3.1.83
6-336

Life Prediction Ratio Summary


a
i

0.

.5

.8

1.25

2.

Ti-6AI-4V
Condition/Ht: MA
Form: Extrusion
Specimen Type: CT
Orientation: LT
Frequency: 6 Hz
Environment: DRY AIR; RT

Yield Strength: 123.5 ksi


Ult. Strength: 135.5 ksi
Specimen Thk: 0.993 - 0.995 in.
Specimen Width: 3.77 in.
Ref: 85837
(3 of 3)

AK (MPaVin)
1

4
10
pri> i i i nil

40

AK (MPaVin)
4
10
i FTTT
Mini

100

40

100

1 ' I Tl'l

10

10
10
10

.22
o
\

o
^10"4
10
-a

10

-J10 >
10
-5

10
10
10
10
4

10

40

'

100

da/dN (10"6in/cycle)

7.05

I I I I II

40

100

da/dN (I0"6in/cycle)

AK (KsiVin)

1.94
5.28
10.3
16.9
45.6
96.0
90.8

10.32 (min)
13.
16.
20.
25.
30.
30.83 (max)

RMS SB
Error

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I I Mil

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


i

0.

2.

Figure 6.16.3.1.83 (Concluded)


6-337

.5

.8

1.25

2.

1 H-6AI-4V I
Condition/Ht: MA
Form: Extrusion
Specimen Type: CT
Orientation: L-T
Frequency: 6 Hz
Environment: DRY AIR; RT

Yield Strength: 122 ksi


Ult. Strength: 139 ksi
Specimen Thk: 0.997 in.
Specimen Width: 4.94 in.
Ref: 85837
(1 of 1)

AK (MPaVin)
4

10

40

AK (MPaVin)
4

100

- I

10

' I 'I'l'l

40

100

' I M'l'l3

10

- Stress Ratio: 0.08

-2

-2

10

10

-i

10

10
:

10

ID"3
~

jo
o
6^10"4
\
c
_

_K
10

io"

o
o^10-4
c
_

-3|
10 E

-3 |

10

Z 10

Z 10
"o

-2

" -*^P
Jio
>

-1.-V

10

10
10

10
10

10

10

10
10

I , I,I,I,

" I , U,l,
4

10

40

-8

10

100

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary

0.

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.175
0.180
0.231
0.340
1.33
4.40
12.6
23.4
31.8
33.7

7.76 (min)
8.
9.
10.
13.
16.
20.
25.
30.
31.20 (max)

RMS %
Error

10

AK (KsiVin)

AK (KsiVin)

15.69

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary

0.

2.

Figure 6.16.3.1.84
6-338

.5

.8

1.25

^ Ti-6AI-4V h
Condition/Ht: MA
Form: Extrusion
Specimen Type: CT
Orientation: L-T
Frequency: 10 Hz
Environment: LAB AIR; RT

Yield Strength:
Ult. Strength:
Specimen Thk: 0.251 in.
Specimen Width: 2 in.
Ref: NC005
(1

AK (MPaVin)
4
10
i I i HIM

of 2)

(2 of 2)

AK (MPaVin)

40
100
1i I M MM

4
10
1 I 1(TI

40
100
. 1 lllM

Stress Ratio: 0.3

-I

10

10
10

10
2
io"

o
:
o^o"4
c

ffl

-3I

10

10

10

10

10

T3

: I

10

10
10

10

40

100

, i.i.i,
4
10

da/dN (I0"6in/cycle)

RMS %
Error
29.84

.5

.8

100

0.0878
0.0802
0.394
8.21
6.36
2.22
3.07
8.82
210.

3.97 (min)
4.
5.
6.
7.
8.
9.
10.
12.66 (max)

Life Prediction Ratio Summary


an
0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.0946
0.259
4.01
18.2
11.9
4.64
11.9
152.
778.

5.10 (min)
6.
7.
8.
9.
10.
13.
16.
16.69 (max)

I,I,I,

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i ,

1.25

RMS %
Error
40.20

Figure 6.16.3.1.85
6-339

Life Prediction Ratio Summary


o

0.

.5

.8

1.25

^ T1-6AI-4V I
Condition/Ht: MA
Form: 1.8 in. Extrusion
Specimen Type: CT
Orientation: LT
Stress Ratio: 0.1
Frequency: 1 10 Hz

Yield Strength: 124.4 ksi


Ult. Strength: 135.3 ksi
Specimen Thk: 1.001 - 1.003 in.
Specimen Width: 4.5 in.
Ref: NC002
(1 of 2)

AK (MPaVin)
4

10

(2 of 2)

AK (MPaVin)
1

40
100
i I M MM

- I

10

' I M'l'l

40

100

' I Tl'l

- Environment: S.T.W.; R.T.

-A 1

-2

10

-1

10
-3

10

2 0)

_Q3

10"

10"

I^-'

6-10-4

o
\

z
^
m" u
u

10

10
10
10
10
-s
10

10

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

60.
66.66 (max)

RMS %
Error
21.82

.5

.8

1.25

40

100

da/dN (10"6in/cycle)
1.62
2.30
4.47
10.9
27.5
53.2
79.7
98.8
210.
727.
779.

10.86 (min)

13.
16.
20.
25.
30.
35.
40.
50.
60.
60.69 (max)

Life Prediction Ratio Summary


an
0.

AK (KsiVin)

1.83
1.87
3.96
11.4
25.6
34.7
46.8
78.9
270.
512.
1477.

10.22 (min)
13.
16.
20.
25.
30.
35.
40.
50.

10

AK (KsiVin)

AK (KsiVin)

2.

RMS %
Error
24.03

Figure 6.16.3.1.86
6-340

Life Prediction Ratio Summary


o

0.

.8

1.25

^ TI-6AI-4V
Condition/Ht: MA
Form: 1.8 in. Extrusion
Specimen Type: CT
Orientation: LT
Stress Ratio: 0.1
Environment: LAB AIR; RT

Yield Strength: 124.4 ksi


Ult. Strength: 135.3 ksi
Specimen Thk: 1 - 1.002 in.
Specimen Width: 4.5 in.
Ref: NC002
(1 of 2)

AK (MPaVin)
1

10

II
= i ' i M'l'ir

40
100
M MIM

10

ni
i ' i 'i'i'ir
10

Frequency: 10. Hz

(2 of 2)

AK (MPaVin)
40
100
i i Min

10

Frequency: 20. Hz

10

-3 I

10

10

10

10

10

40

100

da/dN (10'6in/cycle)

AK (KsiVin)

50.
60.
70.
74.97 (max)

RMS %
Error
6.26

0.

.5

.8

100

1.25

0.540
0.563
3.46
12.2
26.8
42.7
62.3
91.3
226.
702.
1997.

12.95 (min)
13.

16.
20.
25.
30.
35.
40.
50.
60.
67.89 (max)

Life Prediction Ratio Summary


a
i

40

da/dN (10"6in/cycle)

AK (KsiVin)

2.01
3.39
9.35
19.0
31.0
48.5
76.4
189.
453.
1240.
2288.

14.66 (min)
16.
20.
25.
30.
35.
40.

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
20.89

Figure 6.16.3.1.87
6-341

Life Prediction Ratio Summary


CD

0.

.5

.8

1.25

EF

I Ti-6AI-4V r
Condition/Ht: MA
Form: Extrusion
Specimen Type: CT
Orientation: T-L
Stress Ratio: 0.08

Yield Strength: 125 ksi


Ult. Strength: 142 ksi
Specimen Thk: 0.994 in.
Specimen Width: 3.77 in.
Ref: 85837
(1 of 2)

AK (MPaVin)
4

10

' I M'l'l

40

100

b I

' I MTI

Environment: Dry Air; R.T.;


Frequency: 6. Hz

(2 of 2)

AK (MPaVin)
10

' I M'l'l

40

100

TW

T"

-Environment: S.T.W.; R.T.;


_
Frequency: 1. Hz

10

-=j 10

10

10
10

10

10
o

6-10-4

6-10-

10

10

10

-J10 >
"o

XI

_,

10

10
10
-7

10

10

10
10

ILL Ui
4

10

I I II [II
40
100

10

AK (KsiVin)

RMS %
Error
15.22

Life Prediction Ratio Summary


r~

0.

.5

.8

100

1.25

0.428
0.620
1.97
4.67

9.22 (min)
10.
13.
16.
20.
25.
30.
35.
39.27 (max)

1.47
5.48
12.1
16.5
35.4
89.6

13.81 (min)
16.
20.
25.
30.
32.77 (max)

40

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

10

AK (KsiVin)

RMS %
Error
6.87

Figure 6.16.3.1.88
6-342

11.1
24.8
45.1

71.6
98.5

Life Prediction Ratio Summary


-r- -r~

.5

.8

1.25

2.

This page intentionally left blank

6-343

I Ti-6AI-4V I
EF Condition/Ht: MA
Yield Strength: 126.6 ksi
Ult. Strength: 138.6 ksi
Specimen Thk: 1 - 1.003 in.
Specimen Width: 4.5 in.
Ref: NC002

Form: 1.8 in. Extrusion


Specimen Type: CT
Orientation: TL
Stress Ratio: 0.1

(1 of 3)

AK (MPaVin)
4

10

40

100

10

- I ' I M'l'l
Environment: Lab Air- R.T.;
_ Frequency: 5. 20. Hz

~ 10

10

(2 of 3)

AK (MPaVin)
40

100

1 ' I Tl'l

-Environment: S.T.W.; R.T.:


_ Frequency: 1. 10. Hz

"d

10

10
10

-3

10
o
o 10
c

io~2

\
/

-3 |

10

10

10
o
"

-6
10

_A"0

10

10

-5

10

10

10

10

10

-8

10

- i ,.I.I,I,
4

i , I,I,I,

10

40

100

AK (KsiVin)
da/dN (1Cr6in/cycle)

AK (KsiVin)

RMS %
Error
11.93

.5

.8

1.25

40

100

da/dN (10"*in/cycle)
2.30
4.95
11.3
25.9
48.8
66.6
86.0
124.
354.
587.

10.58 (min)
13.
16.
20.
25.
30.
35.
40.
50.
56.74 (max)

Life Prediction Ratio Summary


o
0.

AK (KsiVin)

1.14
2.33
6.65
13.7
23.8
38.5
63.0
103.
277.
865.

11.73 (min)
13.
16.
20.
25.
30.
35.
40.
50.
59.40 (max)

10

AK (KsiVin)

RMS %
Error
18.13

Figure 6.16.3.1.89
6-344

Life Prediction Ratio Summary


o
i

0.

.5 .8

1.25

^ TI-6AI-4V \
Condition/Ht: MA
Form: 1.8 in. Extrusion
Specimen Type: CT
Orientation: TL
Stress Ratio: 0.1

Yield Strength: 126.6 ksi


Ult. Strength: 138.6 ksi
Specimen Thk: 1 - 1.003 in.
Specimen Width: 4.5 in.
Ref: NC002
(3 of 3)

AK (MPaVin)
4

- I

10

' I M'l'l

EF

40
100
li i i i Mil

- Environment: S.S.W.; R.T.:


_
Frequency: 1. - 10. Hz

AK (MPaVin)
4
10
C=II I I I'll

=q
~=\

40

100

' I 'I'M
10

10

10
-3
10
o

O
4

5^ioc

"O

,0-1

_
10

10

10
10
10
10
10
4

10

40

'

100

da/dN (10"6in/cycle)

50.
60.
63.55 (max)

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary

o
0.

100

1.95
4.39
8.83
17.2
31.2
49.1
71.8
102.
209.
560.
899.

10.52 (min)
13.
16.
20.
25.
30.
35.
40.

RMS %
Error
29.88

[ i 11 n

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

.5

.8

RMS %
Error

Life Prediction Ratio Summary


i

0.

1.25

Figure 6.16.3.1.89 (Concluded)


6-345

.5

.8

1.25

\ H-6AI-4V I
Condition/Ht: MA
Form: 4.5 in. Forging
Specimen Type: WOL
Orientation: LT
Frequency: 1 30 Hz
Environment: LAB AIR; RT

Yield Strength: 130 ksi


Ult. Strength: 139 ksi
Specimen Thk: 0.553 - 0.555 in.
Specimen Width: 4.999 - 5 in.
Ref: MA002
(1 of 1)

AK (MPaVin)

AK (MPaVin)
4

4
10
40
100
i i i MIM
IM' I'i'i
10
Stress Ratio: 0.02

10

crii | i |i|i

40

100

' I 'I'I'I

10

10
10

10
10

a;
-2 T;

10

o
o^10-4

10

10* E

10

T3

10

Jio >

10

-S

10

10

10
10

10
10
4

10

40

100

LI

I I I llll
4
10

6.34
8.18
15.7
29.2
53.0
95.0
292.
857.
914.

60.

60.61 (max)

Life Prediction Ratio Summary


i

0.

100

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (I0"6in/cycle)

18.15 (min)
20.
25.
30.
35.
40.
50.

RMS %
Error
12.44

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I l.l.l.

.5

.8

RMS %
Error

Life Prediction Ratio Summary


i

0.

1.25

Figure 6.16.3.1.90
6-346

.5

.8

1.25

H Ti-6AI-4V h
Condition/Ht: MA
Form: 2 in. Forging
Specimen Type: DCB
Orientation: LT
Stress Ratio: 0.02
Frequency: 0.1 Hz

Yield Strength: 145 ksi


Ult. Strength: 156 ksi
Specimen Thk: 0.75 in.
Specimen Width: 5.5 in.
Ref: 84360
(1 of 2)

AK (MPaVin)
1

10

= I ' I 'I'l'l

40

100

1 ' I Tl'l

Environment: Dry Air, R.T.

(2 of 2)

AK (MPaVin)
4

= I
10

10

40

' I 'I'l'l

100

' I 'I'l'l

Environment: Simulated Fuel;


_ R.T.
10

10

10

10
10

-O-

10

_0J

o
6^10"+

o
o 10

_EL

JE

-B-

ho

10
10

Jio >

XI

XJ

XJ

10

10

10

10

10

10

10

10

1A

10

I I II III

10

40

' i iiHI

100

da/dN (10"6in/cycie)

AK (KsiVin)

0.

.5

.8

40

100

RMS %
Error

Life Prediction Ratio Summary


i

1.25

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


i

I I I I III

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error

-5

-5

10

10

10

0.

2.

Figure 6.16.3.1.91
6-347

.5 .8

1.25

H Ti-6AI-4V h
Condition/Ht: MA
Form: 2 in. Forging
Specimen Type: DCB
Orientation: LT
Stress Ratio: 0.02
Frequency: 1 Hz

Yield Strength: 145 ksi


Ult. Strength: 156 ksi
Specimen Thk: 0.75 - 0.875 in.
Specimen Width: 5.5 in.
Ref: 84360

AK (MPaVin)
4
10
40
100

' I M'l'l

1 M'l'l

(1 of 2)

AK (MPaVin)
4
10
40
100

_L

Environment: 3.5 NaCI; R.T. 10

= Environment: Dry Air; R.T.

~~

10

|_

10

10
.-6

10

10.-8

o
\

-5

-3 |

10

- _*"o
10 o

XI

, 1,1,1,

, I,I,I,

10
40
AK (KsiVin)

_,
-6

10

-5

10

10
-6

-= 10

10

Life Prediction Ratio Summary


0.

.8

10
40
AK (KsiVin)

RMS %
Error

Life Prediction Ratio Summary


0.

1.25

Figure 6.16.3.1.92
6-348

100

da/dN (10"6in/cycle)

AK (KsiVin)

.5

1 , 1,1.1,

~ 1 , 1,1,1,

100

da/dN (10"6in/cycle)

AK (KsiVin)

10

RMS %
Error

-2

io ^

z: 10

10

z 10

10

~~

o 10
\
c

10 \
o

10
io"2
o

10

i o-

-2

10

(2 of 2)

.5

.8

1.25

2.

This page intentionally left blank

6-349

I Ti-6AI-4V \~
Condition/Ht: MA
Form: 2 in. Forging
Specimen Type: DCB
Orientation: LT
Stress Ratio: 0.02
Frequency: 10 Hz

Yield Strength: 127 - 145 ksi


Ult. Strength: 139 - 156 ksi
Specimen Thk: 0.75 - 0.875 in.
Specimen Width: 5.5 in.
Ref: 84360
(1 of 4)

AK (MPaVin)
4

= I

10

40

' I 'I'l'l

100

' I 'I'l'l

Environment: Dry Air; R.T.

_ I

100

1 1 llllll

Environment: Dry Argon; R.T.

-3

10

_0)

io" "

o
6-10-4

O
4

frl o"

-3 EI

10

10

2
io" ^

-3 |

-a

-a

10

"o

10

10 \
O
-o

_B I
10

-=: 10

z:

10

10
-7

10

10

-r: 10

10

10

a
10

10

10

40

10

10

-o

10

1 1 'Pill

10

10

(2 of 4)

AK (MPaVin)

" 1 , 1,1,1,
4

1 , 1,1,1,

10

40

10

- 1 , 1,1,1,
4

100

RMS %
Error

da/dN (10_6in/cycle)

Life Prediction Ratio Summary


i

0.

.5

.8

40

100

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

1 , 1,1,1.

10

RMS %
Error

Life Prediction Ratio Summary


i

1.25

da/dN (10"6in/cycle)

AK (KsiVin)

0.

2.

Figure 6.16.3.1.93
6-350

.5 .8

1.25

T;

CAI

' "
Condition/Ht: MA
Form: 2 in. Forging
Specimen Type: DCB
Orientation: LT
Stress Ratio: 0.02
Frequency: 10 Hz

10

(3 of 4)

40

-Ml 'I'l'l
10~

100

' I ' IM1!

_L

10

^^

io'2^
o
\
_3E

O^IO"

Z10"5

10

CD

z.

\
o
"

10"3

10

-6
10

-i

10

^~

10

(4 of 4)

40
100
, 1,,,,,,

I
1
-1
0
Environment: 3.5ss NaCI; R.T. 10

-1

ID"3

4
10
1 11 {I,,!

102

_a>
o

o 10

\
c
^-^
Z10"5

io"2^

a
10

>

\
a
"

"^

-5

10"7
-6

-6

10

10

10

" 1 , 1,1,1,

m"8
1

1C)0

40

RMS s
Error

6
da/dN (10 " in/cycle)

Life Prediction Rati<D Summary


i

0.

.5

.8

I , l.l.i,

10

40

100

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

>

10

I , I , l,l.

10

-6
10

-5

" 1 , 1,1,1,

E
--'
z

T3

ID"7

10

^-8

"' "' 'E

AK (MPaVin)
1

Environment: Distilled Water;


_ R.T.
2

Yield Strength: 127 - 145 ksi


Ult. Strength: 139 - 156 ksi
Specimen Thk: 0.75 - 0.875 in.
Specimen Width: 5.5 in.
Ref: 84360

AK (MPaVin)
1

A\l

da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error

Life Prediction Ratio Summary

1.25

0.

2.

Figure 6.16.3.1.93 (Concluded)


6-351

.5

.8

1.25

2.

i Ti-6AI-4V h
Condition/Ht: MA
Form:
Specimen Type: CT
Orientation: LT
Frequency: 10 Hz
Environment: LAB AIR; RT

Yield Strength:
Ult. Strength:
Specimen Thk: 0.25 - 0.251 in.
Specimen Width: 2 in.
Ref: NC005
(1 of 1)

AK (MPaVin)
4

10

- I ' I M'l'l

40

AK (MPaVin)
1

100

' I M'l'l

Stress Ratio: 0.55

10

t I ' I Tl'l

10

40

100

1 ' I Tl'l

10

-2

10

10

10

10
-3

10
JD

o
\
-3|
10 E

o^10-

.-5

10
XI

10

10

10

_0)

IS

o
6^10-4

,-4

XI

10

o
10

10

10

- f

10

- 1 Tl,l,l,
4

10

I , i.i.i,

10

40

10

'

'

100

da/dN (10*6in/cycle)

AK (KsiVin)

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.356

0.844
1.56
4.56
25.7

6.
7.

8.
8.17 (max)

36.6

Life Prediction Ratio Summary


<m

0.

I I I III

40

0.0159
0.116

3.06 (min)
3.5
4.
5.

r-

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
>100.0

XI

10
10

J2

Z 10

_xT3

10

.5 .8

1.25

RMS %
Error

Life Prediction Ratio Summary


i

0.

2.
Figure 6.16.3.1.94
6-352

.5

.8

1.25

This page intentionally left blank

6-353

^ TJ-6AI-4V
Condition/Ht: MA 1300F 2HRS
Form: 1.75 in. Disk
Specimen Type: KB Bar
Orientation: L-R
Frequency: 0.3 Hz
Environment: LA AIR;300F

AC
Yield Strength: 120 ksi
Ult. Strength:
Specimen Thk: 0.244 - 0.25 in.
Specimen Width: 1 - 1.005 in.
Ref: GE007
(1 of 3)

AK (MPaVin)
4

10

40
1

(2 of 3)

AK (MPaVin)
1

100

' "M'l

10

40

= i ' i Ti'irI

100

' I Tl'l

- Stress Ratio: 0.25

10

-2

10

10
-3

10

JE

-no"2"

_0)

o
o^lO"4
10

10

-Jio >
10
10

10
10
10
4

10

40

100

RMS %
Error
20.55

16.
20.
25.
27.30 (max)

29.8
45.9
82.0
102.

0.

.5

.8

1.25

0.707
3.05
5.14
14.9
26.2
37.5

10.79 (min)
13.

0.649
1.26
2.67
6.90
17.7

Life Prediction Ratio Summary


i

100

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (10-6in/cycle)

10.32 (min)
13.
16.
20.
25.
30.
35.
40.
44.22 (max)

LL

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I I I
40

t mi
10

i-'

2.

RMS %
Error
26.73

Figure 6.16.3.1.95
6-354

Life Prediction Ratio Summary


0.

.5

.8

1.25

H Ti6AI--4^^/
Condition/Ht: MA 1300F 2HRS
Form: 1.75 in. Disk
Specimen Type: KB Bar
Orientation: LR
Frequency: 0.3 Hz
Environment: LAB AIR;300F

AC
Yield Strength: 120 ksi
Ult. Strength:
Specimen Thk: 0.244 - 0.25 in.
Specimen Width: 1-1. 005 in.
Ref: GE007
(3 of 3)

AK (MPaVin)
4

- I

10

40

' I 'I'l'l

AK (MPaVin)

Stress Ratio: 0.54


""~

- I

100

' I 'I'l'l

10

10

io"

Q)

c
^-<-

2M0"5
T3

10

10

E
N_x

-z.

2 10"5
10

T3

4"

wr
jm

io" ^

(0

<D

o
\

10

io-3

<u

10"2

ID"3

-6
10

40

-1

"

10

' I 'I'l'l

10

ID"2

100

' I M'l'l

I
' P

>
T)

10

r?
"a

",-
10
-5

10

10

io-7

ID"7

-6

-6

10

10

"1,1 ,1,1,

m-8

m"8 "

I , l,M,

10

40

100

da/dN (10"6in/cycle)

7.74 (min)
8.
9.
10.
13.
16.
19.93 (max)

RMS %
Error
43.65

,40

100

6
da/dN (10 " in/cycle)

AK (KsiVin)

0.526
0.612
0.868
1.12
4.23
8.63
20.0

Life Prediction Ratio Summary


0.

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , l,l,l,

I , I, I,I,

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary

0.

2.

Figure 6.16.3.1.95 (Concluded)


6-355

.5

.8

1.25

2.

Ti-6AI-4V h
Condition/Ht: MA 1300F 2HRS
Form:
Specimen Type: KB Bar
Orientation: L-R
Frequency: 0.3 Hz
Environment: LAB AIR;600F

- I

10

Yield Strength: 120 ksi


Ult. Strength:
Specimen Thk: 0.249 - 0.253 in.
Specimen Width: 0.995 - 1.003 in
Ref: GE007

(1 of 3)

AK (MPaVin)
1

AC

40
100
i I i | 1111

' I 'I'l'

(2 of 3)

AK (MPaVin)
4

10

40

100

b I ' I 'I'I'lI ' I Tl'l

Stress Ratio: 0
-2

10

-3

10
O

Z 10
a

\
o
"

-6

10

10

10
4

10

40

100

AK (KsiVin)
AK (KsiVin)

41.78 (max)

RMS %
Error
21.59

Life Prediction Ratio Summary


0.

.8

1.25

100

0.898

8.78 (min)
9.
10.
13.
16.
20.
25.
28.82 (max)

1.59
2.25
4.13
7.90
16.2
41.5
89.4
147.
176.

16.
20.
25.
30.
35.
40.

40

da/dN (10-6in/cycle)

AK (KsiVin)

da/dN (10"6 in/cycle)

10.19 (min)
13.

10

AK (KsiVin)

RMS %
Error
22.81

Figure 6.16.3.1.96
6-356

0.995
1.37

2.06
3.76
12.3
27.9
43.4

Life Prediction Ratio Summary


r-

0.

.5

.8

1.25

\ Ti-6AI-4V h
Condition/Ht: MA 1300F 2HRS
Form:
Specimen Type: KB Bar
Orientation: LR
Frequency: 0.3 Hz
Environment: LAB AIR;600F

AC

Yield Strength: 120 ksi


Ult. Strength:
Specimen Thk: 0.249 - 0.253 in.
Specimen Width: 0.995 - 1.003 in
Ref: GE007
(3 of 3)

AK (MPaVin)
4

- I

10

' I M'l'l

40

AK (MPaVin)
4

100

' I M'l'l

Stress Ratio: 0.54

- I

10

' I 'I'l'l

40

100

' I M'l'l

10
10

10

10

10

10

"*

10"
o
\

-3 |

10

o
6^10-4
\
c
_

-3 I

10

:
10

Z 10

10

"D

"O

_K I
10

10

10
10

10

10

-= 10
-8

10

10

-A-O

10

o
-a

- 1 , 1,1,1,
4

1 1,1,1,

10

40

10
4

100

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)
8.13 (min)
9.
10.
13.
16.
20.
20.36 (max)

RMS %
Error
25.57

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.658
0.952
1.46
4.76
12.4
31.1
33.2

Life Prediction Ratio Summary


0.

10

AK (KsiVin)

.5

.8

RMS %
Error

Life Prediction Ratio Summary

0.

1.25

Figure 6.16.3.1.96 (Concluded)


6-357

,
.5

,
.8

!
1.25

I TI-6AI-4V
Condition/Ht: RA
Form: 1.5-2 in. Plate
Specimen Type: CT
Orientation: L-T
Frequency: 6 Hz
Environment: DRY AIR; RT

Yield Strength: 113 - 121 ksi


Ult. Strength: 127 - 135 ksi
Specimen Thk: 0.99 - 1 in.
Specimen Width: 7.4 - 7.41 in.
Ref: 88579;85837
(1 of 4)

AK (MPaVin)
4

10

40

i | i | i[il

1r

- I

10

40

100

' I MTI
10

10

40

100

da/dN (1CT6in/cycle)

AK (KsiVin)

0.141
0.205
0.391
0.778
1.46
4.92
8.52
13.3
27.9

6.12 (min)
7.
8.
9.
10.
13.
16.
20.
25.
25.92 (max)

0.0177

0.0181
0.0486
0.113
0.234
0.437
1.81
4.64
10.1
18.4

31.0

29.9
47.4
71.9
204.
372.

Life Prediction Ratio Summary


A

o OCX

r~

0.

100

AK (KsiVin)

da/dN (10*6in/cycle)

5.98 (min)
6.
7.
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
50.
52.96 (max)

RMS %
Error
36.17

40

' I M'l'l

AK (KsiVin)
AK (KsiVin)

10

Stress Ratio: 0.3

- Stress Ratio: 0.08

100
rrrrrj-

(2 of 4)

AK (MPaVin)

.5

.8

1.25

RMS %
Error
17.77

Figure 6.16.3.1.97
6-358

Life Prediction Ratio Summary


a
o
,

0.

.5

.8

r-

1.25

2.

H TJ-6AI-4V h
Condition/Ht: RA
Form: 1.5-2 in. Plate
Specimen Type: CT
Orientation: LT
Frequency: 6 Hz
Environment: DRY AIR; RT

Yield Strength: 113 - 121 ksi


Ult. Strength: 127 - 135 ksi
Specimen Thk: 0.99 - 1 in.
Specimen Width: 7.4 - 7.41 in.
Ref: 88579;85837
(3 of 4)

AK (MPaVin)
4

10

40

100

10

40

10

100

I1 ' I 'I'l'l

^ I ' I 'I'l'l
Stress Ratio: 0.5

(4 of 4)

AK (MPaVin)

10

Stress Ratio: 0.7

10

10
-1

10

10

-3

10

10

_0>

_a>
o
4

10

6^1 o"

G^10-

10

10

10

10

-Jio
\

"

10

-6 10
10

10

10

10

10

10

10

I , I,I,I,

" I , I,I,I,
4

10

40

da/dN (10"6in/cycle)

RMS %
Error
18.14

,__

0.361
0.775
1.42
2.25

6.
7.
8.
9.
10.
13.
16.
19.21 (max)

2.16

5.09
8.33
18.1
18.2

Life Prediction Ratio Summary

0.

100

0.159

5.11 (min)

1.21

9.
10.
13.
16.
20.
20.65 (max)

'I

da/dN (10"sin/cycle)

AK (KsiVin)

0.292
0.353
0.628

6.39 (min)
7.
8.

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i i i in
4
10

10

100

.5

.8

1.25

2.

RMS %
Error
5.80

14.6
33.6

Life Prediction Ratio Summary


a
r-

0.

Figure 6.16.3.1.97 (Concluded)


6-359

3.21
7.23

.5

.8

1.25

2.

Condition/Ht: RA
Form: 1.5 in. Plate
Specimen Type: CT
Orientation: L-T
Frequency: 1 Hz
Environment: S.T.W.; RT

Yield Strength: 118 ksi


Ult. Strength: 129 ksi
Specimen Thk: 0.995 - 0.998 in.
Specimen Width: 7.4 in.
Ref: 85837
(1 of 3)

AK (MPaVin)
4

10

40

(2 of 3)

AK (MPaVin)
1

100

10

40

ET"' ITI'I

-rrryrr

100

I ' I 'I'M

i ill y

\ TI-6AI-4V I

Stress Ratio: 0.3


-2

10

10

10
10
~~

o
6-10-4
_

10

_fi
10

10

c
Z 10
-o

-5

rh

10

10
10
.-8

10
4

10

40

RMS %
Error
11.85

.5

.8

100

1.25

0.434
0.754
1.39
2.20
7.72

7.37 (min)
8.
9.
10.
13.
16.
20.
22.54 (max)

0.400
0.642
1.19
4.49
10.5
22.4
41.2
62.1
86.2
119.
255.
602.
1055.

Life Prediction Ratio Summary


0.

40

da/dN (10-6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

8.35 (min)
9.
10.
13.
16.
20.
25.
30.
35.
40.
50.
60.
66.77 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , I,I,I,

~ I , I,I,I,

RMS %
Error
10.05

Figure 6.16.3.1.98
6-360

15.5
24.1
27.8

Life Prediction Ratio Summary

0.

1i

.5

.8

1.25

2.

I Ti-6AI-4V
Condition/Ht: RA
Form: 1.5 in. Plate
Specimen Type: CT
Orientation: LT
Frequency: 1 Hz
Environment: S.T.W.; RT

Yield Strength: 118 ksi


Ult. Strength: 129 ksi
Specimen Thk: 0.995 - 0.998 in.
Specimen Width: 7.4 in.
Ref: 85837
(3 of 3)

AK (MPaVin)
1

10

40

b I I 'I'l'l

AK (MPaVin)
1

100

1 ' I Tl'l

- I

="

10

' I' I'l'l

40

100

' I 'I'l'l

10

-2

10

10
-3

10
O

(0

2
10" o
o
\

O 10

\
c

10"

''

z: 10

m
"O

'1
1"

\
u
D

10
-5

10
10
10

10
4

10

40

100

AK (KsiVin)

100

0.272
0.284
0.731
1.24
2.14
4.18

5.97 (min)
6.
7.
8.
9.
10.
13.
16.
17.45 (max)

RMS %
Error
10.63

40

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycie)

AK (KsiVin)

10

AK (KsiVin)

13.6
24.8
29.3

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

RMS %
Error

Life Prediction Ratio Summary


0.

Figure 6.16.3.1.98 (Concluded)


6-361

.5

.8

1.25

i-'

2.

H Ti-6AI-4V h
Condition/Ht: RA
Form: 1.5 - 2.5 in. Plate
Specimen Type: CT
Orientation: LT
Stress Ratio: 0.08
Frequency: 1 Hz

Yield Strength: 118 - 124 ksi


Ult. Strength: 129 - 138 ksi
Specimen Thk: 0.99 - 1 in.
Specimen Width: 7.4 in.
Ref: 85837;88579

AK (MPaVin)
4
10
40
100
-1

I I I l|l|

I- I " M I'M
Environment: Dry Air; R.T.

(1 of 3)

(2 of 3)

AK (MPaVin)
1

= I

33

10

' I M'l'l

40
100
li I i I Mil

Environment: JP-4 Jet Fuel;


R.T.

10

-=\ 1

10

10

10

10
10

10
2

10"

10

10

^10"4

10

-5

10

10

L"0

10

o
10

10

-5

10

10
10

10
-6

10

10
' i i 11 n

' i i i HI
4
10

10

40

10

i i 11 ii

100

da/dN (10_6in/cycle)

AK (KsiVin)
25.
30.
35.
40.
41.69 (max)

.5

.8

100

0.111

7.83 (min)
8.
9.
10.
13.
16.
20.
25.
26.71 (max)

Life Prediction Ratio Summary


0.

i i 11 ii

40

da/dN (10"6in/cycle)

AK (KsiVin)

15.5
16.5
31.7
49.2
75.1
86.7

24.00 (min)

'

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
3.31

io"2
U

o
^10"4

_2

1.25

RMS %
Error
17.85

Figure 6.16.3.1.99
6-362

0.130
0.306
0.637

3.06
7.07
12.4
20.4
25.2

Life Prediction Ratio Summary


0.

.5

.8

1.25

^ Ti6AI-4V r
Condition/Ht: RA
Form: 1.5 - 2.5 in. Plate
Specimen Type: CT
Orientation: LT
Stress Ratio: 0.08
Frequency: 1 Hz

Yield Strength: 118 - 124 ksi


Ult. Strength: 129 - 138 ksi
Specimen Thk: 0.99 - 1 in.
Specimen Width: 7.39 - 7.4 in.
Ref: 85837;88579
(3 of 3)

AK (MPaVin)
4
10
I I 11 ll'l

AK (MPaVin)
1

40
100
1I I 111111

4
10
crii I i Mill

40
100
1i I i |i|i|
10

10
10
10

frio"4
10

10

-o
o

Z 10

XI

10
10
10

10
10
4

10

40

'

100

da/dN (10"6in/cycle)

Life Prediction Ratio Summary

Error

29.82

0.

LL

I I 11 ll

40

100

AK (KsiVin)

da/dN (10-6in/cycle)

0.328
0.359
1.40
3.08
8.22
27.1
57.3
106.
153.

9.87 (min)
10.
13.
16.
20.
25.
30.
35.
37.05 (max)

RMS %

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I I I III

.5

.8

RMS %
Error

Life Prediction Ratio Summary


r~

0.

1.25

Figure 6.16.3.1.99 (Concluded)


6-363

1.25

^ TI-6AI-4V h
Condition/Ht: RA
Form: 1.5 in. Plate
Specimen Type: CT
Orientation: LT
Stress Ratio: 0.08
Frequency: 6 Hz

Yield Strength: 118 - 121 ksi


Ult. Strength: 129 - 134 ksi
Specimen Thk: 0.99 - 0.997 in.
Specimen Width: 5 - 7.4 in.
Ref: 85837:88579
(1 of 2)

AK (MPaVin)
1

10

b I ' I 'I'l'l

40

100

1 ' I Tl'l

Environment: Dry Air; -65T

(2 of 2)

AK (MPaVin)
4
=

10

40

' I 'I'l'l

100

' I 'I'l'l

Environment: Dry Air; 265F

10
10

10

10

10

10

10
2

_aj

io" ^
o
\

b^io-

10

o
\

_
4

O-10c

10

10

^io"2

-3 |

"o

-=j 1

10

-o

_K

10

10

o
-u

-s

_K
10

10

-5

10

10
-7

10

10

10

10
' I iih
4
10

10

l.l.l
40

100

16.
20.
25.
30.
31.93 (max)

RMS %
Error
4.97

0.

.5

.8

1.25

2.44
5.63
10.8
23.1
35.8
44.6

16.
20.
25.
30.
32.07 (max)

Life Prediction Ratio Summary


r~

100

14.47 (min)

1.93
2.37
5.81
10.5
21.4
36.8
40.2

13.

40

da/dN (10_6in/cycle)

AK (KsiVin)

da/dN (1(T6in/cycle)

12.57 (min)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , III 111

II

10

RMS %
Error
4.42

Figure 6.16.3.1.100
6-364

Life Prediction Ratio Summary


a
,

0.

.5

.8

1.25

^ TI-6AI-4V r
Condition/Ht: RA
Form: 1.5-2 in. Plate
Specimen Type: CT
Orientation: LT
Stress Ratio: 0.08
Frequency: 0.1 1 Hz

Yield Strength: 117 - 122 ksi


Ult. Strength: 133 - 135 ksi
Specimen Thk: 0.988 - 1.01 in.
Specimen Width: 7.39 - 7.4 in.
Ref: 88579;85837
(1 of 2)

AK (MPaVin)
1

b I

10

40

' I 'I'l'l

100

' I 'I'l'l

(2 of 2)

AK (MPaVin)
4

10

40

100

I I 'I 'I'l'lI ' I 'I'l'l

- Environment: S.T.W.; 150T

10

-2

10

10
10
o
_
6-10-4
c
_
a

10

10

-5

r=Jl0 >
-o

10

a
10

10
10

10

40

100

AK (KsiVin)

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error
20.11

0.

1.35
1.93
5.61
9.73
28.1
66.3
85.2

76.9

Life Prediction Ratio Summary


i

da/dN (10"6in/cycle)

AK (KsiVin)
12.49 (min)
13.
16.
20.
25.
30.
34.28 (max)

0.585
0.707
2.18
5.44
12.9
24.3
43.0

9.52 (min)
10.
13.
16.
20.
25.
30.
33.81 (max)

i i i im
40
100

I I I Mil
4
10

10

.5

.8

1.25

2.

RMS %
Error
26.14

Figure 6.16.3.1.101
6-365

Life Prediction Ratio Summary

o
0.

I-

-I-

.5

.8

1.25

^ Ti-6AI-4V fCondition/Ht: RA
Form: 1.5 - 2.5 in. Plate
Specimen Type: CT
Orientation: TL
Frequency: 6 Hz
Environment: DRY AIR; RT

Yield Strength: 121 - 122 ksi


Ult. Strength: 134 - 135 ksi
Specimen Thk: 0.99 - 1.013 in.
Specimen Width: 7.38 - 7.4 in.
Ref: 88579:85837
(1 of 2)

AK (MPaVin)
4

10

40

(2 of 2)

AK (MPaVin)
4

100

10

40

_ I 1 I 'nil
1
Stress Ratio: 0.5

l Mill

100

1 1 llllll

-I
10

10

10

10

o^10-4
~
c
_

o
\
-3 |

10

Z 10

T3

10

10
-7

10

10
.-8

10
4

10

40

- i ,

100

da/dN (10"6in/cycle)

RMS %
Error
44.61

.8

1.25

1.48
2.99
5.78

13.
15.81 (max)

r- -T-

.5

100

11.70 (min)

Life Prediction Ratio Summary


o
0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.287
0.295
0.457
1.60
4.40
11.3
21.6
31.8
48.2
82.1
233.
544.
785.

8.94 (min)
9.
10.
13.
16.
20.
25.
30.
35.
40.
50.
60.
63.39 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

1 , 1,1,1,

I,I,I,

2.

RMS %
Error
10.53

Figure 6.16.3.1.102
6-366

Life Prediction Ratio Summary

0.

.5

.8

1.25

Ti6AI-4V
Condition/Ht: RA
Form: 1.5 - 2.5 in. Plate
Specimen Type: CT
Orientation: T-L
Stress Ratio: 0.08
Frequency: 1 Hz

Yield Strength: 122 - 126 ksi


Ult. Strength: 134 - 135 ksi
Specimen Thk: 0.994 - 1 in.
Specimen Width: 7.4 in.
Ref: 85837:88579
(1

AK (MPaVin)
4

10

40

- I I I 'I'l'l

100

I ' I 'I'l'l

of 2)

4
10
i min

-1
10
-

Environment: JP4 Jet Fuel;


_ R.T.

(2 of 2)

AK (MPaVin)
40
100
1i i i iiiM

- Environment: S.T.W.; R.T.

10

10

_0)

~**

2
io~

o
\

O 10
c

-3 |

10

10

10

10

10

10

10

10

1 , 1,1,1,

~ 1 , 1,1,1,
4

10

40

100

da/dN (I0~6in/cycle)

AK (KsiVin)

0.692
3.76
7.32

14.9
20.7

Life Prediction Ratio Summary

0.

.5 .8

40

100

1.25

da/dN (10"6in/cycle)

AK (KsiVin)

0. ,0881
0, .177
0, .326
0. ,541
0, ,832
2 ,26
4. .77
10. 5
23. 2
45. 9
83. 0

6.08 (min)
7.
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
50.
60.
70.
71.06 (max)

0.244
0.245
0.356

7.99 (min)
8.
9.
10.
13.
16.
20.
24.76 (max)

RMS %
Error
10.46

10

AK (KsiVin)

AK (KsiVin)

2.

RMS %
Error
41.07

Figure 6.16.3.1.103
6-367

137.

295.
552.
1325.
1488.

Life Prediction Ratio Summary


-EX A
o
i

0.

.5

.8

1.25

2.

EF

I Ti-6AI-4V I
Condition/Ht: RA
Form: 0.38 - 1.5 in. Plate
Specimen Type: CT
Orientation: TL
Stress Ratio: 0.08

Yield Strength: 125 - 129 ksi


Ult. Strength: 135 - 140 ksi
Specimen Thk: 0.41 - 0.501 in.
Specimen Width: 7.4 in.
Ref: 85837;88579
(1 of 2)

AK (MPaVin)
4
10
pr-ii I i |i|i
TT
-2

40
I

100

- I

I I I'HI

10

Environment: Dry Air; R.T.;


Frequency: 6. Hz

(2 of 2)

AK (MPaVin)
10

i I M'l'l

40

100

' I M'l'l

Environment: S.T.W.; R.T.;


_ Frequency: 1. Hz

10

10

10

10

10

_0J

io'2^

o^10-4

^io"

\
c

-3 |

l_

10

-s

Z 10

10

"a

-6-

10

10

Jio
>

10

-7

10

10

10
10

10
4

10

40

"

100

I , LI,I,

I , I,I,I,

40

da/dN (10"6in/cycle)

RMS %
Error
14.04

6.
7.
8.
9.
10.
13.
16.
20.
23.65 (max)

Life Prediction Ratio Summary


r-

.5

.8

1.25

0.225
0.262
0.437
0.747
1.26
2.08
7.51
19.9
48.7
81.2

5.67 (min)

17.2
27.4

0.

da/dN (10"6in/cycle)

AK (KsiVin)

0.315
0.425
2.58
6.03
10.8

9.68 (min)
10.
13.
16.
20.
25.
29.94 (max)

100

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

RMS %
Error
23.04

Figure 6.16.3.1.104
6-368

Life Prediction Ratio Summary


i

0.

.5

r-

.8

1.25

\ Ti-6AI-4V \
Condition/Ht: RA
Form: 1.5 in. Plate
Specimen Type: CT
Orientation: T-L
Stress Ratio: 0.08

Yield Strength: 117 ksi


Ult. Strength: 133 ksi
Specimen Thk: 1.38 in.
Specimen Width: 4 in.
Ref: 88579

AK (MPaVin)
4

10

40

TTTl

EF

of 1)

AK (MPaVin)
1

100

10

40

b I ' I M'l'l

1 ' I M'l'l

100

1 ' I 'I'll=1

10

Environment: F.C.S.; R.T.;


Frequency: 1. Hz

10

10

10

10

10
10

10

-j

6^10"

Z. 10

-5

10

-3 I

10

-5

-A.-0

10

o
6-10-4
_c
_

io"2

10

10

10

10

10
10

10

10

10
i ' i m

10

I I I III
LJJLL

'

10

40

10

da/dN (10"6in/cycle)

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


0.

. I.I.I

3.62
4.34
9.10
16.4
25.8
26.4

13.81 (min)
16.
20.
25.
30.
30.21 (max)

RMS %
Error
2.42

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I I I 111

100

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


T-

0.

2.

Figure 6.16.3.1.105
6-369

.5

.8

1.25

I TJ-6AI-4V h
EF Condition/Ht: RA

Yield Strength: 141.7 - 149.2 ksi


Ult. Strength: 151.8 - 156.2 ksi
Specimen Thk: 0.372 - 0.375 in.
Specimen Width: 2.549 - 2.55 in.
Ref: 90981

Form: 0.38 in. Plate


Specimen Type: CT
Orientation: TL
Stress Ratio: 0.1

(1 of 2)

AK (MPaVin)
4

\= I

10

40
100
-ii l i I MM

' I 'I'l'l

t= I

10

' I 'I'l'l

40

100

' I 'I'l'l

Environment: S.T.W.; R.T.;


Frequency: 0.1 Hz

10

Environment: Lab Air; R.T.;


Frequency: 10. Hz

(2 of 2)

AK (MPaVin)

10

10

-1

10
-3

10

O
4

frio"

-3 I

10

10

-Jio >

o
10

10
10
10
' i i i in
4
10

10
4

10

40

100

AK (KsiVin)

AK (KsiVin)

35.
36.63 (max)

RMS SB
Error

7.37

Life Prediction Ratio Summary

0.

.5

1405.
1418.
1800.
2531.
3951.
4043.

29.01 (min)
30.
35.
40.
50.
52.51 (max)

5.31
11.3
23.5
39.0
90.6
204.
253.

13.05 (min)
16.
20.
25.
30.

da/dN (10-6in/cycle)

AK (KsiVin)

da/dN (10*6in/cycle)

AK (KsiVin)

i I iI Hi
40
100

.8

1.25

2.

RMS %
Error
14.17

Figure 6.16.3.1.106
6-370

Life Prediction Ratio Summary


o
0.

.5

.8

1.25

TI-6AI-4V h
Condition/Ht: RA
Form: 0.13 in. Plate
Specimen Type: CCP (max load specified)
Orientation: T-L
Frequency: 10 Hz
Environment: H.H.A.; RT

10

10

40

4
10
=|i | i | i|H

100

da/dN (10"6in/cycle)

RMS %
Error
6.15

Life Prediction Ratio Summary


i

.5 .8

10

40

100

1.25

da/dN (10"6in/cycle)

AK (KsiVin)

0.301

4.86 (min)
5.
6.
7.
8.
9.
10.
13.
16.
20.
22.81 (max)

2.21
2.75
3.86
7.21
11.4
22.1
52.3
115.
207.
365.
513.

8.50 (min)
9.
10.
13.
16.
20.
25.
30.
35.
40.
42.13 (max)

40
100
1i I i I il'l

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

(2 of 2)

AK (MPaVin)
1

100

' "Tl

40

Yield Strength: 149.1 - 149.2 ksi


Ult. Strength: 156.2 ksi
Specimen Thk: 0.124 - 0.125 in.
Specimen Width: 5 in.
Ref: 90981

(1 of 2)

AK (MPaVin)

2.

RMS %
Error
12.10

Figure 6.16.3.1.107
6-371

0.335
0.670
1.19

1.90
2.74
3.66
7.71
19.6

65.8
171.

Life Prediction Ratio Summary

0.

.5

.8

1.25

2.

] Ti-6AI-4V \
Condition/Ht: RA
Form: 0.38 in. Plate
Specimen Type: CCP (max load specified)
Orientation: TL
Frequency: 10 Hz
Environment: H.H.A.; RT
(1 of 2)

AK (MPaVin)
4

10

Yield Strength: 141.7 ksi


Ult. Strength: 151.8 ksi
Specimen Thk: 0.37 - 0.371 in.
Specimen Width: 5 in.
Ref: 90981

40
100
1i I i MIM

- I ' I Tl'l

(2 of 2)

AK (MPaVin)
10

40

100

I Tl'l

10

Stress Ratio: 0.1


10

10
10

J2

_
V.-4

o 10
c

10

-Jio >

-5

"O

10

_e ~

10
10
-7

10

10
.-8

10

i i 11 ii

10

I I III!

40

100

AK (KsiVin)

RMS %
Error
4.83

Life Prediction Ratio Summary


a
i

0.

.5

1-i

.8

1.25

100

0.990
1.54

5.41 (min)
6.
7.
8.
9.
10.
13.
16.
20.
23.27 (max)

4.73
6.48
9.13
14.6
23.4
27.1

10.10 (min)
13.
16.
20.
25.
28.25 (max)

40

da/dN (10-6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

10

AK (KsiVin)

2.

RMS %
Error
12.82

Figure 6.16.3.1.108
6-372

2.64
3.85
5.11
6.41

10.9
16.8

26.6
34.9

Life Prediction Ratio Summary


,

0.

.5

.8

r-

1.25

2.

^ TI-6AI-4V r
Condition/Ht: RA
Form: 0.38 in. Plate
Specimen Type: CCP (max load specified)
Orientation: TL
Frequency: 10 Hz
Environment: 3.5$ NACL; RT

Yield Strength: 141.7 ksi


Ult. Strength: 151.8 ksi
Specimen Thk: 0.372 in.
Specimen Width: 5 in.
Ref: 90981

(1 of 2)

AK (MPaVin)
4
10
40 100
1
I 'I'l'lI ' I M'l'l
Stress Ratio: 0.1

AK (MPaVin)
4
10
40 100
1
' M'l'l

10

(2 of 2)

-2

10

10
10

"
v
io~2
o

o
o^lO"4

10
TJ
o

10

-10 >

_. -

10

10
10
-6

10

I , U.L

i i i nn

10

10

40

100

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error
11.36

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

RMS %
Error
17.38

Figure 6.16.3.1.109
6-373

100

da/dN (10"6in/cycle)

AK (KsiVin)

14.4
16.1
20.7
27.2
34.2
51.0
88.0
171.
704.

6.24 (min)
7.
8.
9.
10.
13.
16.
20.
23.07 (max)

37.8
57.5
91.7
128.
177.
208.
202.

17.57 (min)
20.
25.
30.
35.
40.
42.87 (max)

10
40
AK (KsiVin)

Life Prediction Ratio Summary


0.

.5

.8

1.25

^ TJ-6AI-4V
Condition/Ht: RA
Form: 0.13 in. Plate
Specimen Type: CCP (max load specified)
Orientation: T-L
Stress Ratio: 0.1
Environment: 3.5% NACL; RT
(1 of 2)

AK (MPaVin)
4

10

40

100

da/dN (10"6in/cycle)

RMS %
Error
9.49

Life Prediction Ratio Summary


T

0.

.5

.8

1.25

100

' I M'l'l

10

40

AK (KsiVin)

100

da/dN (10-6in/cycle)
2.25
2.73
4.91
15.9
32.4
61.3
110.
173.
249.
314.
332.

8.72 (min)
9.
10.
13.
16.
20.
25.
30.
35.
40.
42.50 (max)

2.00
2.47
3.50
9.45
21.1
44.7
74.0
79.4

8.36 (min)
9.
10.
13.
16.
20.
25.
26.41 (max)

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

h= I ' I ' I'l'l

=q

(2 of 2)

AK (MPaVin)
1

40
100
i I i I >l>l

10

Yield Strength: 149.2 ksi


Ult. Strength: 156.2 ksi
Specimen Thk: 0.125 in.
Specimen Width: 5 in.
Ref: 90981

2.

RMS %
Error
8.34

Figure 6.16.3.1.110
6-374

Life Prediction Ratio Summary


r~

0.

.8

1.25

This page intentionally left blank

6-375

^ Ti-6AI-4V r
Condition/Ht: RA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: TL
Stress Ratio: 0.
Frequency: 15 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(1 of 3)

AK (MPaVin)
1

10

40

|_

100

b I ' I 'I'l'l J ' I 'I'l'l


Environment: Distilled Water;
R.T.

(2 of 3)

AK (MPaVm)
10

40

I 'I'l'l

100

' I 'I'l'l

- Environment: 3.555 NaCI; R.T. 1

10

10

10

-i

-1

10

10

-3

10

10

^Jio"2

_0)

(J

o
o 10

O-10-

10" E

-3 |

10

-5

TJ

10

10

_Jio \

10
10

10

10

10
10

10

10

10
-8

10

'

I Hill

10

40

10

I I MM

i i

100

Life Prediction Ratio Summary


.5

.8

1.25

l i I'll

40

100

da/dN (1Cr6in/cycle)
0.293
0.430
0.630
2.63
3.24

8.60 (min)
9.
10.
13.
13.55 (max)

0.241
0.434
1.32

9.44 (min)
10.
11.75 (max)

10

AK (KsiVin)

da/dN (1CT6in/cycle)

AK (KsiVin)

MM

AK (KsiVin)

AK (KsiVin)

RMS %
Error
11.97

RMS %
Error
8.71

Figure 6.16.3.1.111
6-376

Life Prediction Ratio Summary


7

.5

.8

1.25

i-'

2.

Ti-6A!-4V r
Condition/Ht: RA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: T-L
Stress Ratio: 0.
Frequency: 15 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(3 of 3)

AK (MPaVin)
1

10

40

AK (MPaVin)
4

100

b I ' I 'I'l'lI ' I Tl'l


-Environment: S.T.W.; R.T.

10

TTTl
~d

40

100

' I 'I'l'l

10

10

-2

10

10

10

10
-3

10

10

io"2

_0)

o
\

o
o 10

o
6^10-+

-3 |

10

10

10
-o

Z10
-a

_x"0

10
10

10

10

10
i i 11 HI
40
100

i i i nn
4
10

10

i i i nn
4

da/dN (1CT6in/cycle)

AK (KsiVin)

10

I I llll

40

100

AK (KsiVin)

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

0.365
0.646
2.09

9.40 (min)
10.
12.61 (max)

RMS %
Error
17.28

o
o

10
10

10

-A.T>

10

_
10

Life Prediction Ratio Summary


r

0.

.5

.8

RMS %
Error

Life Prediction Ratio Summary


i

0.

1.25

Figure 6.16.3.1.111 (Concluded)


6-377

-1

.5

.8

1.25

^ T1-6AI-4V
Condition/Ht: RA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: TL
Stress Ratio: 0.1
Frequency: 0.1 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(1 of 5)

AK (MPaVin)
4

- I

10

' I M'l'l

40

' I 'I'l'l

10

10

10

2 10
"o

_K
10

-7

10

10

"

jW

M
rJ

ff

100

Environment: Dry Air; R.T.

_L

10

-i
10

-3 |
10 E

-2

40
T

100

I ' I I I' I

Environment: Water Saturated


_
JP-4 Jet Fuel; R.T.

I , I , l,l.

! I 1 I ill

10

40

--3

10
O

6-10-4

10
o

-o

10
_K

10

10

10
10

10

'

10

.5

.8

1.25

i i 11 n

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

39.1
46.5
73.2
93.7
216.
491.
1567.
4895.

28.99 (min)
30.
35.
40.
50.

60.
70.
79.39 (max)

Life Prediction Ratio Summary


0.

10

AK (KsiVin)

103.
225.
572.
914.

62.76 (max)

i i 11 ii

100

28.5
36.5
66.4

60.

10

da/dN (10-6in/cycie)

27.66 (min)
30.
35.
40.
50.

E
T3

AK (KsiVin)
AK (KsiVin)

10

10

-ZZ 10

RMS %
Errpr
4.09

10

rrrr
' I 'I'l

10

Jio
>
zz

(2 of 5)

AK (MPaVin)

RMS %
Error
13.27

Figure 6.16.3.1.112
6-378

Life Prediction Ratio Summary


.5

.8

1.25

4 T;
Condition/Ht: RA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: TL
Stress Ratio: 0.1
Frequency: 0.1 Hz

10

(3 of 5)

40

- I 'I 'I'l'l

I ' I Tl'l

10"2

10

\
o

-6

10

2
10

>
T3

-S

m"8 ~

i, i,i,i,

10

40

1C)0

RMS %
Error
10.54

-5

10

-6

10

.5

.8

I , I,I,I.

1 , 1,1,1,
4

10

,40

100

1.25

6
da/dN (10 " in/cycle)

AK (KsiVin)
26.28 (min)
30.
35.
40.
50.
60.
70.
75.42 (max)

3 68
6 74
22 5
40 4
59 8
96 4
154
270
428
1327
7237

Life Prediction Rati<o Summary


0.

>

AK (KsiVin)

6
da/dN (10 " in/cycle)

14.90 (min)
16.
20.
25.
30.
35.
40.
50.
60.
70.
78.93 (max)

E
'
z.
x>

AK (KsiVin)
AK (KsiVin)

10

-6

10

~ I , I,I,I,

,-v

"^

io"7

10

10

"-"
Z10"5
-a
\

o
"O
-6 ~"
10

10

o 10

10

m"8

10

io-7

m0

io'3 ~

_3E

JJP

2 10-5

"O

-i

10

^^

100

' 1 ' I'l'l

Environment: 3.5 NaCI; R.T

J~

-2

j*

o 10

40

Q>

JKf

10

- 1 ' I ' I'l'l


10

Iif

ID"3

1
_L

t*J

''

(4 of 5)

AK (MPaVin)

100

Environment: Distilled Water;


_ R.T.

4.V 1I
TV

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140

AK (MPaVin)
1

AI_

2.

RMS %
Error
16.28

Life Prediction Rati o Summary


0.

Figure 6.16.3.1.112 (Continued)


6-379

321
697
928
1173
2144
2469
8074
9712

.5

.8

1.25

2.

^ TI-6AI-4V r
Condition/Ht: RA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: T-L
Stress Ratio: 0.1
Frequency: 0.1 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(5 of 5)

AK (MPaVin)
4

10

40
1

b I ' I 'I'l'l

AK (MPaVin)
1

100
1

I 'IT

- Environment: S.T.W.; R.T.

10

- i i 'i'l'l

40

100

nTri'i

-1

-2

10

10
10

-3

10

10

io"

_0J

o
fri o"4

<o

10
o
\

10~

Q)

6^10-4
c

zio

10
10

"O

10 \
u
u

10
10

10
10

10

10

10
' i ' i in

i !!

10

40

10
4

100

da/dN (10"6in/cycie)

AK (KsiVin)

Life Prediction Ratio Summary


i

0.

40

100

AK (KsiVin)

da/dN (10*6in/cycle)

179.
260.
507.
821.
2088.
2106.

30.23 (min)
35.
40.
50.
60.
60.36 (max)

12.35

10

AK (KsiVin)

AK (KsiVin)

RMS SB
Error

^^

z
P

10

10

.5

.8

RMS %
Error

Life Prediction Ratio Summary


ii

0.

1.25

Figure 6.16.3.1.112 (Concluded)


6-380

.5 .8

1.25

i-'

2.

TI-6AI-4V h
Condition/Ht: RA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: T-L
Stress Ratio: 0.5
Frequency: 0.1 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(1 of 5)

AK (MPaVin)
4
1

10

I M'l'l

40

= I

' I M'l'l

10

40

100

da/dN (I0"6in/cycle)

9.
10.
13.
16.
20.
25.
30.
31.84 (max)

RMS %
Error
16.54

1.08
2.57
6.86
20.4
48.6
70.2
72.2

10

40

100

1.25

da/dN (10"6in/cycle)

AK (KsiVin)

12.1
12.2
17.2
35.1
71.4
136.

35.
40.

274.
2017.

46.00 (max)

Life Prediction Ratio Summary

.8

100

' I 'I'l'l

15.67 (min)
16.
20.
25.
30.

0.930
0.930

8.99 (min)

40
I

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

' I M'l'l

Environment: Water Saturated 10


_
JP-4 Jet Fuel; R.T.

10

Environment: Dry Air; R.T.

100

(2 of 5)

AK (MPaVin)

2.

RMS S
Error
9.48

Figure 6.16.3.1.113
6-381

Life Prediction Ratio Summary


-r-

.5

1.25

H T1-6AI-4V h
Condition/Ht: RA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: TL
Stress Ratio: 0.5
Frequency: 0.1 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(3 of 5)

AK (MPaVin)
4

10

40
I

' I M'l'l

100

10

40

100

i ' i 'I'llr

-iI I I inn

I 11IIM

Environment: Distilled Water;


_ R.T.

(4 of 5)

AK (MPaVin)

-Environment: 3.5 NaCI; R.T. -d 10

-d 10
10

10

-1

10

10
-3

10

10

io"

-3 I

10

io"2

o
o 10

-3 |

10

10

10

10

o
~

.-6

10

=j10 >
-o

-6
10

^
10

10

10

10
-6

10

10

Li'

.-8

10

Li Hi

10

40

10

100

i i i i in
4
10

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

0.998
1.01
1.42
2.03
5.75
14.5
40.2

7.97 (min)
8.
9.
10.
13.
16.
19.93 (max)

9.39
12.2
21.8
43.4
117.
391.
1347.
1411.

14.81 (min)
16.
20.
25.
30.
35.
40.
40.19 (max)

da/dN (10_6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

i i i nil
40
100

AK (KsiVin)

AK (KsiVin)

RMS %
Error
11.14

2.

RMS %
Error
22.59

Life Prediction Ratio Summary


0.

Figure 6.16.3.1.113 (Continued)


6-382

.5

.8

1.25

J
Condition/Ht: RA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: TL
Stress Ratio: 0.5
Frequency: 0.1 Hz

- I

10

(5 of 5)

40

' I 'I'l'l

' I 'I'l'l

_i

10

- I

io-3

100

' I ' I'l'l

io"

o
\
-3|
10 E

o
^io"4
\
c

zio'5

Z10"

\
o

10

a;

io"2

o
\
-3|
10 v E
'

-z.

T3

>

66

10

T>
-5

-5

10

10
-

io"7

io"7
-6

-6

10

10

I , LI,!,

10

6
da/dN (10 " in/cycle)

Life Prediction Rati<D Summary


i

12.42

0.

40

100

6
da/dN (10 " in/cycle)

AK (KsiVin)

77 7
160
209
262

22.18 (min)
25.
30.
34.79 (max)

RMS %
Error

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , M.l,

" I , I,1.1,

m"8
1

H)0

40

>

~ .**
10

io

-1

N x

TJ

,-' "i.i ,i,i,

10

10

<D

v_^

"

' I ' I'l'l

40

io"3

<D

10

-1

10

I
.
I p.

io"2

^10"
\
c

ID'2

0)

A\l
tv

AK (MPaVin)
1

100

Environment: S.T.W.; R.T.


_

__

CAL

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140

AK (MPaVin)
1

T;

1-

.5

.8

RMS %
Error

Life Prediction Rati D Summary

1.25

0.

2.

Figure 6.16.3.1.113 (Concluded)


6-383

.5

.8

1.25

2.

^ TI-6AI-4V hCondition/Ht: RA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: TL
Stress Ratio: 0.5
Frequency: 1 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(1 of 6)

AK (MPaVin)
4
10
prii i 111 F

40
100
1> I i HIM

i- i

10

40

' i M'l'i

100

r
. VTT~

Environment: Water Saturated


JP-4 Jet Fuel; R.T.

10

Environment: Dry Air; R.T.

(2 of 6)

AK (MPaVin)

10

-2

10

-3

10
O

5M 0"+

10

10

10
10.-8
4

10

40

100

AK (KsiVin)

13.
16.
20.
25.
30.
35.
37.05 (max)

RMS %
Error
11.40

Life Prediction Ratio Summary


i

0.

.5 .8

1.25

100

0.774
0.943
1.55
4.49
9.27
19.1
37.0
60.0
112.
327.
2981.

8.65 (min)
9.
10.
13.
16.
20.
25.
30.
35.
40.
45.45 (max)

1.74
4.95
9.60
18.2
33.6
63.8
171.
267.

10.40 (min)

40

da/dN (10-6in/cycle)

AK (KsiVin)

da/dN (10'6in/cycle)

AK (KsiVin)

10

AK (KsiVin)

i-

2.

RMS %
Error
16.68

Figure 6.16.3.1.114
6-384

Life Prediction Ratio Summary


,

0.

.5

.8

1.25

2.

Ti-6AI-4V
Condition/Ht: RA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: TL
Stress Ratio: 0.5
Frequency: 1 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(3 of 6)

AK (MPaVin)
4

= I

10

' I 'I'l'l

40

100

10

40

I- I

1i I i I MM

Environment: Alternate JP-4


Jet Fuel and Distilled Water;
R.T.

10
|_

RMS 95
Error
23.26

40

-=| 10

100

37.8
49.5
77.9
168.
349.

1.25

0.475
1.29
2.77
9.43
16.6
28.0
49.3
82.5
147.
372.
3246.

9.
10.
13.
16.
20.
25.
30.
35.
40.
44.64 (max)

1.17

r~

da/dN (I0"6in/cycle)

8.08 (min)

1.66
6.23
18.4

.8

10

AK (KsiVin)

0.985
0.986

.5

100

AK (KsiVin)

Life Prediction Ratio Summary


0.

40

' I 'I'l'l

Environment: Distilled Water;


R.T.

100

da/dN (10"6in/cycle)

7.94 (min)
8.
9.
10.
13.
16.
20.
25.
30.
35.
39.99 (max)

10

' I 'I'l'lI

AK (KsiVin)
AK (KsiVin)

(4 of 6)

AK (MPaVin)

RMS %
Error
29.23

Life Prediction Ratio Summary


0.

Figure 6.16.3.1.114 (Continued)


6-385

,
.5

,
.8

,
1.25

2.

\ Ti-6AI-4V r
Condition/Ht: RA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: T-L
Stress Ratio: 0.5
Frequency: 1 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(5 of 6)

AK (MPaVin)
4

10

40

C=1' I i Ml'

' I M'l'l

Environment: 3.5s? NaCI; R.T.

100

10

40

4
10
=|i | i | i|i|

100

RMS %
Error
22.38

Life Prediction Ratio Summary


0.

.5

.8

40

AK (KsiVin)

100

da/dN (10-6in/cycle)
1.26
2.01
9.57
26.0
51.3
88.7
160.
235.
377.
406.

9.27 (min)
10.
13.
16.
20.
25.
30.
35.
40.
40.49 (max)

0.946
1.08
2.67
20.4
65.4
115.
147.
261.
464.
698.
2388.

10

AK (KsiVin)

da/dN (10"6in/cycle)

8.86 (min)
9.
10.
13.
16.
20.
25.
30.
35.
40.
44.53 (max)

40
100
1i I ' I MM

10

AK (KsiVin)
AK (KsiVin)

(6 of 6)

AK (MPaVin)

1.25

RMS %
Error
9.34

Life Prediction Ratio Summary


0.

Figure 6.16.3.1.114 (Concluded)


6-386

i-'

r-

.8

1.25

2.

This page intentionally left blank

6-387

i Ti-6AI-4V h
Condition/Ht: RA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: T-L
Stress Ratio: 0.5
Frequency: 1 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(1 of 4)

AK (MPaVin)
4
10
fzr-Ti I i Mil

IT

40
100
I I 11 >MI

Environment: Dry Air; 175F

10

40
100
1i I i |ilH

I ' I Tl'l

(2 of 4)

AK (MPaVin)
Environment: JP-4 Jet Fuel;
175T

10

-2

10

10

10

10

10
-3

10

10

(O

2
10~ o
o
\

_0)

_Q3
U

o
\

O 10
10

10

6^10-4
c.

-Z. 10

..x>
10

X>

10"

-5

o
XI

XI

_K

'\
u
x>

10

10
10

10

10

10
' i i i in

i I i III
4
10

40

'

10

100

.5

.8

1.25

100

10.7
16.7
27.4
40.7
63.2
110.

16.60 (min)
20.
25.
30.
35.
40.
45.72 (max)

Life Prediction Ratio Summary


0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

5.45
6.24
13.9
23.6
46.1
66.0
97.7
156.

15.65 (min)
16.
20.
25.
30.
35.
40.
42.30 (max)

10

AK (KsiVin)

da/dN (l0-6in/cycle)

AK (KsiVin)

' i i im

I I I Ml

AK (KsiVin)

RMS %
Error
7.82

t"

10

10

10

2.

RMS %
Error
6.58

Figure 6.16.3.1.115
6-388

215.

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

H Ti-6AI-4V h
Condition/Ht: RA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: TL
Stress Ratio: 0.5
Frequency: 1 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(3 of 4)

AK (MPaVin)
1

10

40

100

b I ' I 'I'l'lI ' I 'I'll


Environment: Distilled Water;
175F

(4 of 4)

AK (MPaVin)
4

10

= I ' I 'I'l'l
10

40

100

I ' I 'I'l'l

-Environment: 3.5* NaCI; 175T-=j 10


10
10
10
JQJ

io"2
o

o 10
c

-Aio E,
z:
-Jio >

|_
10

-5

T3

10
10
-7

10

10

10

40

100

da/dN (10"6in/cycle)

RMS 55
Error
6.23

Life Prediction Ratio Summary


i

0.

.5

.8

40

100

1.25

da/dN (10"6in/cycle)

AK (KsiVin)

41.8
326.
416.
474.
786.
1507.
3196.

16.62 (min)
20.
25.
30.
35.
40.
46.18 (max)

12.7
15.0
29.8
43.2
60.3
94.7
168.
304.

15.44 (min)
16.
20.
25.
30.
35.
40.
44.48 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I.I.I.

' I ' I III

10
4

i-'

2.

RMS %
Error
33.19

Life Prediction Ratio Summary


i

0.

Figure 6.16.3.1.115 (Concluded)


6-389

.5 .8

1.25

i-

2.

-{ TI-6AI-4V hCondition/Ht: RA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: T-L
Stress Ratio: 0.5
Frequency: 1 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(1 of 1)

AK (MPaVin)
1

=
-2

10

40

AK (MPaVin)
4

100

i i M'l'ii ' i TI;I

Environment: Nitrogen & Air;


_ -65F

t=1i

10

I > |i|>

40
100
Ii I i I Mil
10

10
^

10

10

10

10
-3

10

_0)

ju
I

6^10-4
c
"O
XI

-3 I

10

10

10

o
_
O-10-4

-5

-Jio >

XI
o

_R -

10

r-

10

-Jio >

-s
D

_K

10

10

10

10
-7

10

10

10

10

I I.U.

10

i l.l.l

10

40

10

I . i.u
4

100

da/dN (10-6in/cycle)

Life Prediction Ratio Summary


i

da/dN (10"6in/cycle)

AK (KsiVin)

6.45
11.5
23.0
36.0
82.3
218.

17.05 (min)
20.
25.
30.
35.
39.00 (max)

RMS X
Error
11.50

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i ' iin
40
100

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary

I--

0.

2.

Figure 6.16.3.1.116
6-390

.5

.8

1.25

i-'

2.

H Ti-6AI-^VJ

Condition/Ht: RA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: TL
Stress Ratio: 0.8
Frequency: 1 Hz

Ei

10

(1 of 1)

40

' I Tl'l

' I Tl'l

4
_

_i

10

10

| ,,.,.,

40
|

100

| ,,,,,,

10

IQ"3

a>

^10"
c

io"
o

0)

10-3P
E

rf

-1

10

io-3

a>

<o
2

io"

u
o 10

-3IE

10

Z10"5

X)

\
o

\
D

-8
106

-i

10

-1

Z10"5

10"2

"

AK (MPaVin)
1

100

Environment: Dry Air; R.T.

IQ"2

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140

AK (MPaVin)
1

II

10

>

10

&

-5

-5

10

10

io"7

IQ"7

-6

-6

10

10

10

IC)0

40

- 1 , 1,1,1,

m"8

I , 1,1,1,

irC*

RMS %
Error

6
da/dN (10 " in/cycle)

Life Prediction Ratk3 Summary


i

0.

.5

40

100

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , l.l.l,

10

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


0.

2.

Figure 6.16.3.1.117
6-391

da/dN (10"6in/cycle)

AK (KsiVin)

.5

.8

1.25

2.

^ Ti-6AI-4V F
Condition/Ht: RA
Form: 0.38 in. Plate
Specimen Type: PTSF (max stress specified)
Orientation: LS
Stress Ratio: 0.1
Frequency: 10 Hz
(1 of 1)

AK (MPaVin)
4

10

Yield Strength: 119.1 ksi


Ult. Strength: 138.1 ksi
Specimen Thk: 0.376 in.
Specimen Width: 5 in.
Ref: 90981

AK (MPaVin)
1

40
100
i I i I i|i|

- I ' I 'IT

b= I

10

40

' I M'l'lI

100

' I Tl'l

Environment: H.HA; R.T

10

10
10
-3

10

J2

.2>
o
6^10-4

10
10

_^"
10

10
10
10
10

10
4

10

40

'

LL

100

da/dN (10'6in/cycle)

100

da/dN (10-6in/cycle)

AK (KsiVin)

0.789
1.11
3.02
6.66
12.8
19.3
24.2
30.9
35.6

Life Prediction Ratio Summary


0.

LJiii
I I
40

0.676

8.50 (min)
9.
10.
13.
16.
20.
25.
30.
35.
37.14 (max)

RMS %
Error
11.89

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I I 11 ll

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


I--

i-'

0.

2.

Figure 6.16.3.1.118
6-392

.5

.8

1.25

2.

^ Ti-6AI-4V h
Condition/Ht: RA
Form: 0.38 in. Plate
Specimen Type: PTSF (max stress specified)
Orientation: TS
Stress Ratio: 0.1
Frequency: 10 Hz

Yieid Strength: 141.7 ksi


Ult. Strength: 151.8 ksi
Specimen Thk: 0.377 in.
Specimen Width: 5 in.
Ref: 90981

(1 of 1)

AK (MPaVin)

AK (MPaVin)
4

4
10
40
100
I I 11 Mil
I I M III
IT
- Environment: 3.5* NaCI; R.T. -=\ 10

10

I M'l'l

40

100

' I M'l'l

10

10

10

10

10
10

10

3
o

O 10
10

m
10

6-10-4
c
_

10

-o

TD

10

10"2
o

10

-5

\
o

73

-6

10

10

10
-5

10

10
-7

10

10

10

10
I I I I III
4
10

10

10

40

da/dN (I0"6in/cycle)

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

37.3
37.9
49.7
67.2
84.6
99.2
101.

15.77 (min)
16.
20.
25.
30.
35.
35.80 (max)

RMS %
Error
22.73

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

' i i i in

' i i im

100

Life Prediction Ratio Summary


i

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary

i-'

r-

2.

0.

.5

.8

Figure 6.16.3.1.119
6-393

1.25

] TI-6AI-4V I
Condition/Ht: RA
Form: 4 in. Forging
Specimen Type: CT
Orientation: L-T
Frequency: 6 Hz
Environment: DRY AIR; RT

Yield Strength: 121 ksi


Ult. Strength: 132 ksi
Specimen Thk: 1 in.
Specimen Width: 7.4 in.
Ref: 88579
(1 of 2)

AK (MPaVin)
4

10

40
100
i I I I i Ml

10

40

RMS %
Error
11.95

36.1

Life Prediction Ratio Summary

0.

.5

40

100

da/dN (1CT6in/cycle)
0.770
1.16
4.53
8.92
15.5
27.2
45.9
74.5
120.
339.
579.

9.44 (min)
10.
13.
16.
20.
25.
30.
35.
40.
50.
57.20 (max)

14.0
23.7

3494 (max)

10

AK (KsiVin)

0.169
0.621
1.98
6.58

16.
20.
25.
30.

40
100
i I i I MM

AK (KsiVin)

da/dN (1Cr6in/cycle)

10.40 (min)
13.

10

100

AK (KsiVin)
AK (KsiVin)

(2 of 2)

AK (MPaVin)

.8

1-25

2.

RMS %
Error
6.62

Figure 6.16.3.1.120
6-394

Life Prediction Ratio Summary


a
.5

.8

1.25

This page intentionally left blank

6-395

H TI-6AI-4V r
Condition/Ht: RA
Form: 4 in. Forging
Specimen Type: CT
Orientation: LT
Stress Ratio: 0.08
Frequency: 1 Hz

Yield Strength: 121


Ult. Strength: 132
Specimen Thk: 0.9
Specimen Width: 6
Ref: 88579
(1 of 3)

AK (MPaVin)
1

- I

10

40

I 'I'l'l

' I Tl'l

(2 of 3)

AK (MPaVin)
1

100

Environment: Dry Air; R.T.

- 123 ksi
- 136 ksi
- 1 in.
- 7.4 in.

- I
10
-2

10

40

' I 'I'l'l

100

' I 'I'l'l

Environment: JP-4 Jet Fuel;


_
R.T.

10

10

10
-3

10

U
4

o^10-

10

10
10

10
10
10
10
'

10
4

10

40

100

RMS %
Error
26.35

16.
20.
25.
30.

0.834
2.01
5.83
16.3
34.4
58.5
86.9
173.
321.

0.

.5

r-

.8

1.25

100

0.682
0.727
1.51
4.95

12.53 (min)
13.

0.355
0.392

15.3
26.5
28.2

32.23 (max)

Life Prediction Ratio Summary


o
i

40

da/dN (10-6in/cycle)

AK (KsiVin)

da/dN (I0"6in/cycle)

9.37 (min)
10.
13.
16.
20.
25.
30.
35.
40.
50.
58.69 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , l.l.l

I I I 111

2.

RMS %
Error
22.61

Figure 6.16.3.1.121
6-396

Life Prediction Ratio Summary


a
I--

-I-

.5

.8

1.25

2.

I Ti-6AI-4V r
Condition/Ht: RA
Form: 4 in. Forging
Specimen Type: CT
Orientation: LT
Stress Ratio: 0.08
Frequency: 1 Hz

Yield Strength: 121


Ult. Strength: 132
Specimen Thk: 0.9
Specimen Width: 6
Ref: 88579
(3 of 3)

AK (MPaVin)
4

10

40

TTTT

AK (MPaVin)
1

100

10

40

b I ' I ' I'll

' I M'l'l

- Environment: S.T.W.; R.T.

- 123 ksi
- 136 ksi
- 1 in.
- 7.4 in.

100

I ' I 'I'l'l

10

10

10

10

10
-3

10

10

io"2 P

.>
I
o
6^10-4

10

-5

10

10

XJ

XI

_-

10

XJ

10

10

10
-7

10

10

10
10

10
4

10

40

'

100

da/dN (10"6in/cycle)

100

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


a
0.

40

0.376
0.395
0.553
0.902
1.58
7.93
18.7
38.8
44.1

6.72 (min)
7.
8.
9.
10.
13.
16.
20.
21.08 (max)

RMS %
Error
6.92

10

I I I I ll

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'

I I I 111

.5

.8

1.25

RMS %
Error

2.

Life Prediction Ratio Summary


i

0.

.5

.8

Figure 6.16.3.1.121 (Concluded)


6-397

1.25

2.

i TI-6AI-4V I
Condition/Ht: RA
Form: 4 in. Forging
Specimen Type: CT
Orientation: TL
Frequency: 6 Hz
Environment: DRY AIR; RT

Yield Strength: 119 - 128 ksi


Ult. Strength: 127 - 136 ksi
Specimen Thk: 1 in.
Specimen Width: 7.4 in.
Ref: 88579
(1 of 2)

AK (MPaVin)
1

b I

10

40

' I 'I'l'l

(2 of 2)

AK (MPaVin)
4

100

' I 'I'l'l

10

40

100

Stress Ratio: 0.5

"3 10

-3 10

10"2^

10

10

10
o
6^10-4
c

2 10
"""""
-o

T3

_fi|
10
10
:
10

10
10

10

40

100

i , i .i.i.

I , LLL

40

da/dN (10'6in/cycle)

13.
16.
20.
25.
30.
35.
40.
50.
60.
68.69 (max)

RMS 5*
Error

13.14

0.

.5

.8

1.25

1.98
2.62
6.93
11.5
19.7
33.7
51.2
79.7
105.

9.49 (min)
10.
13.
16.
20.
25.
30.
35.
37.30 (max)

Life Prediction Ratio Summary


-T"

da/dN (1Cr6in/cycle)

AK (KsiVin)

0.819
0.908
2.57
7.57
19.0
33.0
47.9
66.7
137.
317.
940.

12.73 (min)

100

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

RMS %
Error
7.98

Figure 6.16.3.1.122
6-398

Life Prediction Ratio Summary


-r- -r-

0.

.5

.8

1.25

2.

TJ-6AI-4V r
Condition/Ht: RA
Form: 4 in. Forging
Specimen Type: CT
Orientation: TL
Frequency: 1 Hz
Environment: S.T.W.; RT

Yield Strength: 128 ksi


Ult. Strength: 136 ksi
Specimen Thk: 0.66 - 0.77 in.
Specimen Width: 7.4 in.
Ref: 88579
(1 of 2)

AK (MPaVin)
1

10

b I ' I ' I MM

40

100

40

.5

.8

1.25

10

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

1.78
1.78
2.25
3.41
14.3
36.9
58.0
98.6
196.
238.
539.
628.

7.69 (min)
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
40.43 (max)

0.610
0.619
1.74
4.87
14.2
32.2
52.4
77.7
111.
185.
303.

Life Prediction Ratio Summary


0.

40
100
i I i 11111

AK (KsiVin)

da/dN (10"6in/cycle)

9.95 (min)
10.
13.
16.
20.
25.
30.
35.
40.
50.
58.05 (max)

RMS %
Error
13.38

10

100

AK (KsiVin)
AK (KsiVin)

(2 of 2)

AK (MPaVin)

1 ' I Tl'l

10

2.

RMS %
Error
9.35

Figure 6.16.3.1.123
6-399

Life Prediction Ratio Summary

0.

.5

.8

1.25

2.

^ Ti-6AI-4V h
Condition/Ht: RA
Form: 4 in. Forging
Specimen Type: CT
Orientation: TL
Frequency: 1 Hz
Environment: S.T.W.; RT

Yield Strength: 119 - 124 ksi


Ult. Strength: 127 - 136 ksi
Specimen Thk: 0.91 - 1.01 in.
Specimen Width: 6 - 7.4 in.
Ref: 88579
(1 Of 1)

AK (MPaVin)
4

10

AK (MPaVin)
1

40
100
I I I I MM

_ I

10

10

I I llTj

40

100

I I llllll

10

6-10-4

Z10-5

10

10

Q)

10

40

100

I . I,I,I,

I , LI,I,

40

100

AK (KsiVin)

da/dN (10"*in/cycle)

0.203
0.412
0.752
2.87
7.16
16.9
35.8
62.0
95.2
135.
235.
290.

Life Prediction Ratio Summary


o

0.

10

AK (KsiVin)

da/dN (10_*in/cycle)

8.02 (min)
9.
10.
13.
16.
20.
25.
30.
35.
40.
50.
54.52 (max)

RMS %
Error
24.09

03

2
o
^~" 10"
o
\

10" N
'
z

10 \
u
D

10

=1

AK (KsiVin)
AK (KsiVin)

10

10

10

-I

.5

.8

RMS %
Error

Life Prediction Ratio Summary


i

.5

1.25

Figure 6.16.3.1.124
6-400

r-

.8

1.25

2.

Ti-6AI-4V h
Condition/Ht: RA(FAST COOLED)
Form: 1 in. Plate
Specimen Type: DCB
Orientation: TL
Stress Ratio: 0.1
Frequency: 1 Hz
(1 of 1)

AK (MPaVin)
1

- I

10

' I M'l'l

40

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140

AK (MPaVin)
1

100

' I M'l'l

=]

- Environment: 3.5 NaCI; R.T. 1

10

t I ' I 'I'l'l

40

100

1 ' I M'l'l

10

-2

10

10
10
Q)

o
6^10-4
c
_
T3
XI

10

10*
o
\

-3 I

10

-5
-4X>

_fi

10
-5

10
10

-6

10
10
4

10

40

'

' ' "ii

100

da/dN (10"6in/cycle)

13.11

Life Prediction Ratio Summary

0.

100

da/dN (10"6in/cycle)

AK (KsiVin)

15.2
17.2
29.7
52.4
84.0
151.
265.
420.

14.96 (min)
16.
20.
25.
30.
35.
40.
47.90 (max)

RMS %
Error

111in

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'

10

.5

.8

RMS %
Error

Life Prediction Ratio Summary


r-

0.

1.25

Figure 6.16.3.1.125
6-401

i--

.5

.8

1.25

2.

^ TI-6AI-4V h
Condition/Ht: STOA
Form: 0.62 in. Plate
Specimen Type: CT
Orientation: LT
Stress Ratio: 0.3
Frequency: 1 Hz

Yield Strength: 140 ksi


Ult. Strength: 150 ksi
Specimen Thk: 0.491 in.
Specimen Width: 6 in.
Ref: 85837
(1 of 1)

AK (MPaVin)
4

10

40

= I ' I Tl'l

AK (MPaVin)
4

100

I ' I 'I'll

b I

_L

10

40

' I 'I'll

100

' I 'I'l'l

Environment: Dry Air; R.T.


-2

10

10

10

(0

jU

10

10

10

6^10-

-3 |

-5

10

10

10

XI

10

^io~ ^
o

-3 |

10

ZIG"5
\
a
~ -el10

UP*
/

JO
2

v
o
6^10-'
\

10

10

-7

10

10

10

10
10

10

1 , 1,1,1,

" 1 , 1,1,1,
4

10

40

10

100

da/dN (10-6in/cycle)

13.

16.
18.56 (max)

Life Prediction Ratio Summary

0.

LLL

I I I III

40

100

da/dN (10-6in/cycle)

AK (KsiVin)

8.99
9.53
20.1
35.0

11.82 (min)

RMS %
Error
10.07

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'

i i 11 ii

.5

.8

1.25

2.

RMS %
Error

Life Prediction Ratio Summary


i

0.

Figure 6.16.3.1.126
6-402

.5

.8

1.25

H TJ-6AI-4V
Condition/Ht: STRESS RELIEVED E.B. WELDMENT (HAZ)
Form: Weldment
Yield Strength:
Specimen Type: CT
Ult. Strength:
Orientation: T-L
Specimen Thk: 1 in.
Stress Ratio: 0.1
Specimen Width: 2.55 in.
Environment: LAB AIR;-65F
Ref: 88144
(1 of 2)

AK (MPaVin)
1

10

40

i ' i Ti'i

100

10

1i
i ' i 'nir

| I I MM

10

Frequency: 0.1 Hz

(2 of 2)

AK (MPaVin)

40
100
i ' HIM=q
10

Frequency: 10. Hz

-2

10

10

10

10
.-3

10

-B-

10

_03

_0J

o^lO"4

^IO"

10

10"2

10

Z 10

10

T>

10
o

10

10

-5

10

10
10

10

10

10

10

i i i ni

10

,-B

10

l i l 111

40

100

Life Prediction Ratio Summary


i

0.

.5 .8

10

40

100

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

' ' '""

. I.1.1.

AK (KsiVin)

RMS %
Error

T3

XI

_.

1.25

RMS s
Error

Life Prediction Ratio Summary


-r~

0.

2.
Figure 6.16.3.1.127
6-403

da/dN (10"6in/cycle)

AK (KsiVin)

.5

!S

1.25

2.

^ TI-6AI-4V r
Condition/Ht: STRESS RELIEVED E.B. WELDMENT (HAZ)
Form: Weldment
Yield Strength:
Specimen Type: CT
Ult. Strength:
Orientation: T-L
Specimen Thk: 1 in.
Stress Ratio: 0.1
Specimen Width: 2.55 in.
Environment: 3.5 NACL; RT
Ref: 88144
(1 of 2)

AK (MPaVin)

b I
Frequency: 0.1 Hz

10

' I 'I'M

40

100

' I 'I'l'l

10

Frequency: 10. Hz

~
10

10

-3

10

10

10

10

_a>
o

10"

"~"
_

10

Z 10
\

110"

10

Z 10
XI
\
o

X>

"O

Q>

-Jio
>

-6
10

-2

6^10-4

i o-

(2 of 2)

AK (MPaVin)

10

-6

10

10

10
-7

10

II I I

10

-6

10

\
10

10

40

I . KM.

.-8

I , I,I,I,

10

10

100

RMS %
Error
48.35

Life Prediction Ratio Summary


.5

.8

1.25

100

8.64
9.28
24.8
47.3
87.7

19.78 (min)
20.
25.
30.
33.73 (max)

17.1
10.5
152.
2519.
7755.
148646.

r-

40

da/dN (10'6in/cycle)

AK (KsiVin)

da/dN (10"6in/cycle)

22.24 (min)
25.
30.
35.
40.
49.52 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

' I i Uli

RMS %
Error
43.38

Figure 6.16.3.1.128
6-404

Life Prediction Ratio Summary


0.

-1

i-

.5

.8

1.25

2.

^ TI-6AI-4V h

Condition/Ht: STRESS RELIEVED E.B. WELDMENT (HAZ)


Form: Weldment
Yield Strength:
Specimen Type: CT
Ult. Strength:
Orientation: T-L
Specimen Thk: 1 in.
Stress Ratio: 0.1
Specimen Width: 2.55 in.
Environment: JP4; RT
Ref: 88144
(1 of 2)

AK (MPaVin)
4

z. |

10

, | i|in

40

100

i | ipn

-2

100

I I I MM

10

10

10

10

10

-5

40
1

10

o
^10"+

10

Frequency: 10. Hz

10

.2?

-I
>- i i M'l'ir

~= 10

Frequency: 0.1 Hz

(2 of 2)

AK (MPaVin)

10

io"

10"

o^10-+

10"

T3

T5

'

A TJ

.-6

10

-5

""""

'1

4
m \
U

-Jio
>

10

o
\

-z.

3 10

10

-A
10

-7

10

10

10

10
10

- i .

i . i,i,i,

I,I,I,
4

10

40

'

10

da/dN (10"6in/cycle)

RMS %
Error
51.87

Life Prediction Ratio Summary


0.

.5

.8

I ' HU

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

6.05
9.36
17.8
25.7
35.2
60.6
2543.

18.39 (min)
20.
25.
30.
35.
40.
45.20 (max)

6.87
14.6
16.1
19.1
80.1
358.
621.
2893.

18.23 (min)
20.
25.
30.
35.
40.
50.
56.28 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'

I I I I ll

100

1.25

RMS %
Error
37.44

Figure 6.16.3.1.129
6-405

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

^ TI-6AI-4V h
Condition/Ht: STRESS RELIEVED E.B. WELDMENT (HAZ)
Form: Weldment
Yield Strength:
Specimen Type: CT
Ult. Strength:
Orientation: T-L
Specimen Thk: 1 in.
Stress Ratio: 0.1
Specimen Width: 2 in.
Environment: LAB AIR; RT
Ref: 88144
(1 of 2)

AK (MPaVin)
4

10
TTTr

Frequency: 0.1

40
100
TI I I I MM

10

40

= I ' I'l'l'l

100

I ' I Tl'l

Frequency: 10. Hz

10

Hz

(2 of 2)

AK (MPaVin)

10

10
-3

-3

I
j

10

10

o
&1 a"4

o
o^10-4

"F

10 ^E

CD

10

10
10

_.

10~

N x

10 \
u
-o

10
10

-7

10

10

10

10
''I'll
4
10

10

I I I III

40

100

10

40

da/dN (1Cr6in/cycle)

AK (KsiVin)

5.22
5.32
11.3
39.6
92.7
137.
150.
508.
1436.

15.64 (min)
16.
20.

25.
30.
35.
40.
50.
52.34 (max)

Life Prediction Ratio Summary


0.

.5

.8

100

AK (KsiVin)

da/dN (I0"6in/cycle)

AK (KsiVin)

I , LI,I,

- i , i,i,i,

AK (KsiVin)

RMS %
Error

10

.-8

<D

10

XI

_. 10

10

~ 10

10

10

"o

1.25

RMS %
Error
27.00

Figure 6.16.3.1.130
6-406

Life Prediction Ratio Summary


,

0.

.5

.8

1.25

2.

H Ti6AI--4V
Condition/Ht: STRESS RELIEVED E.B. WELDMENT (HAZ)
Yield Strength:
Form: Weldment
Ult. Strength:
Specimen Type: CT
Specimen Thk: 1 in.
Orientation: TL
Specimen Width: 2.55 in .
Stress Ratio: 0.1
Ref: 88144
Environment: 3.5s NACL;175T

(1

AK (MPaVin)
4

- I

10

40

' I 'I'l'l

' I 'I'l'l

__

la'3

of 2)

10

= i

100

' I 'I'l'l

^_^

io"3
(0

10

Z10"

>

**

X)

XI

-6
10

io~2

\
o
"

Z10"

10

X>

-5

-5

10

io"7

10"7
-6

I , l,M,

, I ,l,l,

10

40

-6

10

10

" I , I,I,I,

io"8
1

100

RMS SB
Error

da/dN (10'6in/cycle)

'

I , I .l,l.

10

,40

100

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

>

-6
10 ~~

10

"

*'

m-8

10

10

10

n/cyc

>

n/cyc

' I ' I'l'l

40

io"2

^_^.

\
o
"

10

Frequency: 10. Hz

io-2

1
a

(2 of 2)

AK (MPaVin)

100

Frequency: 0.1 Hz
"

io-2

\j-

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

2.

RMS %
Error

Life Prediction Rati o Summary


0.

Figure 6. 16.3.1.131
6- 407

6
da/dN (10 " in/cycle)

AK (KsiVin)

.5

.8

1.25

2.

^ Ti-6AI-4V r
Condition/Ht: STRESS RELIEVED E.B. WELDMENT (HAZ)
Form: Weldment
Yield Strength:
Specimen Type: CT
Ult. Strength:
Orientation: T-L
Specimen Thk: 1 in.
Stress Ratio: 0.1
Specimen Width: 2.55 in.
Environment: DIST WATER;175F
Ref: 88144
(1 of 2)

AK (MPaVin)
4

-IM

10

'i'i'i

40

100

10

10

10

i i 'i'i'i

-ii I i I i|i|

Frequency: 0.1 Hz

(2 of 2)

AK (MPaVin)
40

100

I ' I 'I'I'I
r

Frequency: 10. Hz

10

-S-

10

10
-3

-3

.EL

10

cP

10

.2*

-lio"2

io"2

fcio"4

o 10
10

-?

io"JE

10

10
10

XI

-6

XJ

XI

Jio >
x

10

10

10

10
10

10

10

10

10.-8

10

I I I I ill

i I iI Hi

10

40

Life Prediction Ratio Summary


i

.5

.8

10

40

100

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

i , i.i ill

I t'l'

100

AK (KsiVin)

RMS %
Error

10

da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error

Life Prediction Ratio Summary


i

0.

1.25

Figure 6.16.3.1.132
6-408

.5

.8

1.25

i-'

2.

^ Ti-6AI-4V r

Condition/Ht: STRESS RELIEVED E.B. WELDMENT (HAZ)


Form: Weldment
Yield Strength:
Specimen Type: CT
Ult. Strength:
Orientation: T-L
Specimen Thk: 1 in.
Stress Ratio: 0.1
Specimen Width: 2.55 in.
Environment: LAB AIR;175F
Ref: 88144
(1 of 2)

AK (MPaVin)
1

- I

10

I I ll'l'l

40

100

' I M'l'l

Frequency: 0.1 Hz

~= 10

10

10

10

-3

10

10

I
4

2
10~

6^10-4

-3 t:
E

10"

10

-Jio
>

-^

4"
\
u

10

10

10

-7

10

10

10

10
10

"O

_c
10

10

(O

wa

-s
10

"o

40
100
I I I Il|i|

10

i a"

10

Frequency: 10. Hz

-2

- i ' i Ti'i

10

-5

(2 of 2)

AK (MPaVin)

I , !,U.

- I , I.I,I,
4

10

40

10
4

100

da/dN (10-6in/cycle)

AK (KsiVin)

10

40

da/dN (10"6in/cycle)

AK (KsiVin)

481
9.03
15.0
21.6
33.1
52.5
119.
1183.
2391.

16.93 (min)
20.
25.
30.
35.
40.
50.
60.
61.62 (max)

RMS %
Error

Life Prediction Ratio Summary


i

0.

.5

.8

100

AK (KsiVin)

AK (KsiVin)

1.25

RMS %
Error
25.08

Figure 6.16.3.1.133
6-409

Life Prediction Ratio Summary


0.

.5

.8

1.25

^ Ti-6AI-4V r
Condition/Ht: STRESS RELIEVED E.B. WELDMENT (WELD ZONE)
Form: Weldment
Yield Strength:
Specimen Type: CT
Ult. Strength:
Orientation: T-L
Specimen Thk: 1 in.
Stress Ratio: 0.1
Specimen Width: 2 in.
Environment: DIST WATER; RT
Ref: 88144
(1 of 2)

AK (MPaVin)
1

- I

10

I 'I'l'l

40

100

- I

' I M'l'l

10

40

'I 'I'l'lI

100

' I 'I'l'l

=*
10

Frequency: 10. Hz

10

Frequency: 0.1 Hz

(2 of 2)

AK (MPaVin)

-2

10

10

10

10
-3

10

10

JO

-jio"2

2u

io"

u
6^10-4

6^10"

- io~J E

10
10

10
o
"

-6

10

10

10

10
10

10
10

10

lil

i i i nil
4

10

40

I I I llll
4
10

10
100

RMS %
Error
>100.0

6497.

Life Prediction Ratio Summary


.5

.8

1.25

7.92
16.5
49.9
160.
1394.
8242.
25779.

25.83 (min)
30.
35.
40.
50.
60.
68.14 (max)

2.92
18.7
127.
588.
4116.

100

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (10'6in/cycle)

25.76 (min)
30.
35.
40.
50.
54.73 (max)

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

40

10

RMS %
Error
94.42

Figure 6.16.3.1.134
6-410

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

i--

2.

H Ti-6AI-4V h
Condition/Ht: STRESS RELIEVED E.B. WELDMENT (WELD ZONE)
Form: Weldment
Yield Strength:
Specimen Type: CT
Ult. Strength:
Orientation: T-L
Specimen Thk: 1 in.
Stress Ratio: 0.1
Specimen Width: 2 in.
Environment: LAB AIR; RT
Ref: 88144
(1 Of 1)

AK (MPaVin)
1

10

=
i ' i M'l'i

40

AK (MPaVin)
1

100

1I I l I MM

= I

10

40

' I 'I'l'lI

100

' I 'I'll

=*

10

Frequency: 10. Hz

10

10

10

10
10

10

u
o 10

o
\
10

52.

io"2^
o
6^10-4

10

-Z. 10

Z 10
o

T3

10

Jio >

T3

.-6

10

10

10

10
10

10

10

10
I

I I I I II
4
10

10

10

I I I I I I

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

25.
30.
35.
40.
40.52 (max)

100

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


i

0.

40

3.36
4.10
10.9
23.8
58.6
197.
925.
1107.

15.48 (min)
16.
20.

RMS %
Error
45.50

10

AK (KsiVin)

AK (KsiVin)

.5

.8

RMS %
Error

Life Prediction Ratio Summary

0.

1.25

Figure 6.16.3.1.135
6-411

.5

.8

1.25

i Ti-6AI-4V h
Condition/Ht: STRESS RELIEVED E.B. WELDMENT (WELD ZONE)
Form: Weldment
Yield Strength:
Specimen Type: CT
Ult. Strength:
Orientation: T-L
Specimen Thk: 1 in.
Stress Ratio: 0.1
Specimen Width: 2.55 in.
Environment: 3.5 NACL; RT
Ref: 88144
(1 of 1)

AK (MPaVin)
1

10

AK (MPaVin)
4

40
100
-1I
I
I
I'l'l^
r

- i ' i 'I'ri

10

40
-l

TT

100
I I MM

10

10

Frequency: 0.1 Hz
-2

10

10

10

10
-3

10

10

io"2

-jio"
o

-3 |

6^10-

10

10

\
o

"

D
10

X>

-sl-

io-4

,o-I

_
10

-5
~

"O

Jio >
-o

_K

10

10

10

10

10

10

10

10
' i i in
40
100

i I iI Mi
4
10

10

JiL

10
4

da/dN (10"6in/cycle)

Life Prediction Ratio Summary


i

89.10

0.

ILL
100

da/dN (10-6in/cycle)

AK (KsiVin)

17.8
120.
854.
2746.
5987.
18134.
20210.

21.95 (min)
25.
30.
35.
40.
50.
51.09 (max)

RMS S3
Error

I I

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

1-i

.5

.8

1.25

RMS %
Error

i--

Life Prediction Ratio Summary


i

0.

2.

Figure 6.16.3.1.136
6-412

.5

.8

1.25

1~'

2.

^ TI-6AI-4V r
Condition/Ht: STRESS RELIEVED E.B. WELDMENT (WELD ZONE)
Form: Weldment
Yield Strength:
Specimen Type: CT
Ult. Strength:
Orientation: T-L
Specimen Thk: 1 in.
Stress Ratio: 0.1
Specimen Width: 2.55 in.
Environment: 3.5* NACL;175F
Ref: 88144
(1 of 2)

AK (MPaVin)
1

- I

10

' I 'I'l'l

40

' I 'I'l'l

Frequency: 0.1 Hz

10

40

100

' I 'I'l'l

10

10
10
2

-4^o

^10'

_Q3

o^10-4

Z. 10
o

tz

- 10" E

10

^Jio >

x>

-3 |

-I io

-J10 >
10

10

10

10

10

I,I,I.
4

10

10

1111 n

40

100

i i iin
4
10

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


i

0.

.5

.8

I I im

40

100

AK (KsiVin)

AK (KsiVin)

RMS %
Error

_e
10

10

10

10

10

10

10

Frequency: 10. Hz

10

-o

= I ' I 'I'l'l
10

-er

-3

(2 of 2)

AK (MPaVin)

100

RMS %
Error

Life Prediction Ratio Summary


i

0.

1.25

Figure 6.16.3.1.137
6-413

da/dN (10"6in/cycle)

AK (KsiVin)

r-

.5

.8

1.25

2.

^ TI-6AI-4V r
Condition/Ht: 1000F 2HR
Form: 2 in. Forging
Specimen Type: TDCB
Orientation: L-T
Yield Strength: 145 ksi
Ult. Strength:

Specimen Thk: 1.25 in.


Specimen Width: 5.5 in.
Ao:
Klscc: 31-43 ksi
Ref: 84360

Kmax (MPaVin)
1

10

-I'l 'I'l'l

40

100

I ' I 'l'l'l

Environment: 3.5ss NaCI

40

100

' I 'I'l'l

Environment: JP-4 Jet Fuel

~ 10

10

10

\
c
.^10"

10

10

1I

2
10

10
-

10

-J10

o
\
i E

| 10

n "O

a
XJ

10

-i

Ill I

-2

10

10

10

I,I,I,
40

10

35.60 (min)
40.
47.00 (max)

I I I

LL

100

10

113.

0
40

100

Kmax (Ksivin)

Kmax (KsiVin)
Kmax (KsiVin)

10

10

i ,

-a

-2

10

10

i~

n -O

10

10

^'1

10

10

10

' I'l'l'l

10

101

-2

10

| io

(2 of 2)

Kmax (MPaVin)

2)

Kmax (KsiVin)

da/dt (I0"3in/hour)
222.
4001.
28004.

RMS %
Error

RMS %
Error
41.5

Figure 6.16.3.2.1
6-414

da/dt (10*3in/hour)

H Ti-6AI-4V h
Condition/Ht: EB WELD STRESS RELIEVED (HEAT AFFECTED ZONE)
Form: Weldment
Specimen Thk: 1 in.
Specimen Type: CT
Specimen Width: 2.55 in.
Orientation: TL
Ac-:
Yield Strength: 132 ksi
Kiscc: 33 ksi
Ult. Strength:
Ref: 88144
(1

Kmax (MPaVin)
4

10

- I 'I 'I'l'l

40

of 2>

100

' I 'l'l'l

10

10-2

~~

o i ,0

10

~
-

T3

10

10

10

,o-i

10

10
c

" 1 , 1,1,1,
4

10

1 , 1,1,1,
40

RMS %
Error

10

_,~o

10

on

zz

10

10

100

I , I,I,I,

I , l.l.l,

40

10

i-

1
,0-f
-2,

-3

10

10

10

10

T3

10
-

1 00

Kmax (Ksivin)

Kmax (Ksivin)
Kmax (KsiVin)

_i

'mtmm

Environment: Air; 175T

10

-^ 10

100

. I llllll

"~"

10

40

*~~ 10

10

I I .III.)

10

PFl

_ I

Environment: 3.5 NaCI; 75T

10

(2 of 2)

Kmax (MPaVin)

da/dt (10"3in/hour)

Kmax (KsiVin)

RMS %
Error

Figure 6.16.3.2.2
6-415

da/dt (10'3in/hour)

H Ti-6AI-4V r
Condition/Ht: EB WELD STRESS RELIEVED (WELD ZONE)
Form: Weldment
Specimen Thk: 1 in.
Specimen Type: CT
Specimen Width: 2.55 in.
Orientation: T-L
Ao:
Yield Strength: 132 ksi
Klscc: 36 - 51.5 ksi
Ult. Strength:
Ref: 88144

Kmax (MPaVin)
4

10

' I 'I'l'l

40

of 2)

(2 of 2)

Kmax (MPaVin)
4

100

10

I MUH

IT

' I 'I'l'l

40

100

I 'I'l'l

Environment: Air; 175T;


_ Klscc=51.5

Environment: 3.3K NaCI; 75T;-=J10


Klscc=36.

10

10

10

10

10

Si
10

10

10"
o

10

10

o i-

10~
\
c
4-10"

II
10

X>

10

-B-

-cr

-2,

O
XI

la"1 1
10

10
10

10
10

10

10

10

I.I,

10
4

10

rf ' ""
4

40

10

100

36.00 (min)
40.
44.00 (max)

10

40

1 oo

Kmax (Ksivin)

Kmax (Ksivin)
Kmax (KsiVin)

I Ml

da/dt (10"3in/hour)

Kmax (KsiVin)

0.197
764.
1001.

RMS %
Error

RMS %
Error
>100.0

Figure 6.16.3.2.3
6-416

da/dt (10"3in/hour)

H Ti-6AI--41{/v
Condition/Ht: MA
Form: 0.2 in. Sheet
Specimen Type: DCB
Orientation: TL
Yield Strength:
Ult. Strength:

- I

10

' I 'I'l'l

40

(1 of 6)
1

' I 'I'l'l

_L

10

Environment: 0.6M KCI


_
-1000MV; R.T.

(2 of 6)

Kmax (MPaVin)

100

= I

10

I 'I'l'l

40

100

' I 'I'l'l

_i10

Environment: 0.6M KCI


_
-500MV; R.T.

102

102

...

101

Jio
\
c
**^s

10')

TJ

10
-2
10

~N

L_

Jio
j.. 10_1

2
-_
,u *-

\
c
cr>

10

101

2
10

io3

\
a
"

Specimen Thk: 0.2 in.


Specimen Width:
Ao:
Kiscc-'
Ref: 81221

Kmax (MPaVin)
1

0 "
\
o
o

m
a

-M IO"'
a
\
o
"
-2
10

"*"

,o'l
N'

10

0 J3
>
o
TJ

-1
10

-1

10
10"3

10"3
-2

io"2

10
m"4
1

I I,I,I,

I , LI,I,

40

10

m"4

_ I , I,I,I,
1

100

23.00 (min)
25.
30.
35.
40.
45.20 (max)

RMS %
Error
13.71

40

100

Kmax (Ksivin)

Kmax (Ksivin)
Kmax (KsiVin)

10

I , l.l.l,

da/dt (10" 3in/hour)

Kmax (KsiVin)
22.00 (min)
25.
30.
35.
40.
45.20 (max)

232.
266.
299.
341.
474.
867.

RMS %
Error
10.48

Figure 6.16.3.2.4
6-417

3
da/dt (10" in/hour)

194.
608.
778.
949.
1096.
1447.

^ TI-6AI-4V h
Condition/Ht: MA
Form: 0.2 in. Sheet
Specimen Type: DCB
Orientation: TL
Yield Strength:
Ult. Strength:

Specimen Thk: 0.2 in.


Specimen Width:
Ao:

isccRef: 81221

(3 of 6)

Kmax (MPaVin)
4

10

40

100

10

b I ' I'l'l'l
~= 10
~

Environment: 0.6M KCI


_ OMV; R.T.

10

__

i-

110

"

-=10

E
10

^J10">

_,
-

T3

10

o
73

-2

10

10

10

10

10

10

-2

10

10
10

10

10

-M10

1 ' I M'l'l

10

10

100

10

-C

40

Environment: 0.6M KCI


+500MV; R.T.

10

10

(4 of 6)

Kmax (MPaVin)

" I IUI!4

10

I , LI,I,
40

100

21.50 (min)
25.
30.
35.
40.
45.00 (max)

10

1 oo

40

Kmax (Ksivin)

Kmax (Ksivin)
Kmax (K sivin)

JJi

I . I.I.I.

10

da/dt (10"3in/hour)

Kmax (KsiVin)
23.00 (min)
25.
30.
35.
40.
45.20 (max)

549.
898.
1264.
1785.
2470.
3072.

RMS %
Error
8.28

RMS %
Error
8.74

Figure 6.16.3.2.4 (Continued)


6-418

da/dt (10"3in/hour)
882.
1236.
1823.
2242.
3027.
5110.

H M-6AI--4V Ii
Condition/Ht: MA
Form: 0.2 in. Sheet
Specimen Type: DCB
Orientation: TL
Yield Strength:
Ult. Strength:

Specimen Thk: 0.2 in.


Specimen Width:
Ao:
KjsccRef: 81221
(5 of 6)

Kmax (MPaVin)
1

10

- I ' I ' I MM

40

100

' I Tl'l

-i

10

Environment: 0.6M KCI


_ +1000MV; R.T.

io2

10

= I ' I 'ITI

40

100

I ' I 'ITI

_L

10

Environment: 0.6M KCI


_ +2000MV; R.T.
3

\
c

If

Jio
^10"1

102

101

Jio
-M 10"'
TJ

"

XJ

-2
10
-i

O,

-2
10

io3

da/dt (mm/hour)

io1

io"3

10
10"3

-2

" I , I,hi,
1

10

i , I.I.I,

io-4 "
1

1C)0

40

23.50 (min)
25.
30.
35.
40.
45.00 (max)

I , I,I,I,

I , I.I.I,

40

10

100

Kmax (KsiVin)

Kmax (KsiVin)
Kmax (KsiVin)

-2

10

10
io"4

102
10

\
o
"

(6 of 6)

Kmax (MPaVin)

3
da/dt (10" in/hour)

Kmax (KsiVin)

403.
1509.
2319.
3450.
5550.
5949.

RMS s
Error

RMS %
Error
12.02

Figure 6.16.3.2.4 (Concluded)


6-419

3
da/dt (10" in/hour)

1 T1-6AI-4V hCondition/Ht: MA
Form: 0.2 in. Sheet
Specimen Type: DCB
Orientation: TL
Yield Strength:
Ult. Strength:

Specimen Thk: 0.2 in.


Specimen Width:
Ao:
Klscc: 35 ksi
Ref: 81221

Kmax (MPaVin)
1

b I

10

' I 'I'l'l

40

100

' I 'I'l'l

-Environment: 1M KF; R.T.

^
~=i

(2 of 4)

Kmax (MPaVin)

4)

10

' I 'I'l'l

40

100

' I 'I'l'l

Environment: 3M KF; R.T.

10

10

10

10

10

10
10

101

10

-J10 i

110

-4 A

-1

^10

*.10_1
-o
\
o
" -2

10

x>

10

\
1 E
E

-H-

tn

1SZ

| io !i
\

10

_,

o
-a

10

10

10

10

10

10"3

10

10
IQ"4

'

I I III'

10

Al
.1 I Mill
0
100
40

10

35.00 (min)
40.
44.20 (max)

RMS *
Error
18.

Mill
10

I l I llll
40
100

Kmax (Ksivin)

Kmax (KsiVin)
Kmax (KsiVin)

Kmax (KsiVin)

da/dt (10"3in/hour)
30.0
207.
529.

RMS 55
Error

Figure 6.16.3.2.5
6-420

da/dt (10"3in/hour)

^ T1-6AI-4V
Condition/Ht: MA
Form: 0.2 in. Sheet
Specimen Type: DCB
Orientation: T-L
Yield Strength:
Ult. Strength:

Specimen Thk: 0.2 in.


Specimen Width:
Ao:
Kiscc: 35 ksi
Ref: 81221
(3 of 4)

Kmax (MPaVin)
1

(4 of 4)

Kmax (MPaVin)
1

10

40
100
1'
.
.I ' .urn
10
Environment: 6M KF; R.T,

10

- I ' I 'I'l'l

- I ' I 'I'l'l

40

100

1 ' I 'I'l'l

Environment: Dist. Water; R.T. -=10

10

10

10

10

10

10
10

,0

k-

'1

SZ

sz 10
\

10

\
1 E
E

^ 10

10

10
"o

| 10
\
c

_,
10

tZ

10

a
10

10

10
10

10

-2

-2

10

10
' i i i in

10

10

' i i mi

40

i i i mi

10

100

30.00 (min)
35.
40.
44.50 (max)

RMS %
Error
11.91

40

100

Kmax (Ksivin)

Kmax (KsiVin)
Kmax (KsiVin)

10

i i i mi

da/dt (10"3in/hour)

Kmax (KsiVin)
31.40 (min)
35.
40.
45.00 (max)

461.
1075.
2121.
3590.

RMS %
Error
3.87

Figure 6.16.3.2.5 (Concluded)


6-421

da/dt (10"3in/hour)
196.
381.
485.
522.

^ Ti-6AI-4V h
Condition/Ht: MA
Form: 0.2 in. Sheet
Specimen Type: DCB
Orientation: T-L
Yield Strength:
Ult. Strength:

Specimen Thk: 0.2 in.


Specimen Width:
Ao:
KjsccRef: 81221

Kmax (MPaVin)
4

b I

10

' I'l'l'l

40

(2

Kmax (MPaVin)

6>

100

' I'l'l'l

-Environment: 5M Kl -1500MV; 10
_
R.T.

4
10
40
100
I I i Ml
I ' I 'I'l'l
-Environment: 5M Kl -1000MV; 10
_ R.T.
10

10
10

10

10

=)

110

-=n

10 2

*-

1 E

10

tr-

1-

-M10"'

.^10
XJ

-2
10

-a
\
o
"

10

-2
10

-1

10

10

a
-3

10

10

10

10
10

6)

10

10

\
o
~

I I I'll
410

Li

i i mi

10

< i 11 HI

JO 100
4C
Kmax (KsiVir
(Ksivin)

Kmax (KsiVin)

10

i i i Mi

40

100

Kmax (KsiVin)
Kmax (KsiVin)

da/dt (10-3in/hour)

30.00 (min)
35.
40.
44.00 (max)

RMS 5?
Error
7.12

RMS s
Error

Figure 6.16.3.2.6
6-422

da/dt (10"3in/hour)
1237.
2496.
9603.
10002.

H Ti-6AI-4^JV
Condition/Ht: MA
Form: 0.2 in. Sheet
Specimen Type: DCB
Orientation: TL
Yield Strength:
Ult. Strength:

Specimen Thk: 0.2 in.


Specimen Width:
Ao:
KisccRef: 81221
(3 of 6)

Kmax (MPaVin)
1

= I

10

' I 'I'l'l

40

I ' I 'ITI

_i

10

10

10
-

10

??

_C

__ ,0')

10

T
ffl

2 '^

+.10"1
\
o
"

100

F
10'

40

102

JP

10
\
c

10

HM

i_
3

- Environment: 5M Kl 0MV;
_ R.T.

102

or
T\

(4 of 6)

Kmax (MPaVin)

100

- Environment: 5M Kl -500MV
_ R.T.

101

II

-zz.

i_

1U 2

T
ITI

3
a
10
\

10

>
-o

-2
10

10' I
^S
4-*

"--*
10

-1

10

IQ"3

-2

-2

10

10

" I , I.I.I,
1

10

I , I,I,I,
40

- I , I,I,I,

in"4
1

100

19.20 (min)
20.
25.
30.
35.
40.
44.70 (max)

RMS %
Error
17.77

10

I , 1.1,1.
40

100

Kmax (Ksivin)

Kmax (Ksivin)
Kmax (KsiVin)

>
~o

-1

m"4

10

10
IQ"3

-C

-M 10
TJ

""

3
da/dt (10" in/hour)

Kmax (KsiVin)
18.50 (min)
20.
25.
30.
35.
40.
44.80 (max)

1390.
2779.
11081.
13644.
22181.
33262.
33578.

RMS %
Error
15.94

Figure 6.16.3.2.6 (Continued)


6-423

da/dt (10"3in/hour)
1355.
5587.
16341.
24942.
44033.
61104.
59957.

^ TI-6AI4V h
Condition/Ht: MA
Form: 0.2 in. Sheet
Specimen Type: DCB
Orientation: TL
Yield Strength:
Ult. Strength:

Specimen Thk: 0.2 in.


Specimen Width:
Ao:

KlsccRef: 81221

4-10

b I

' I 'I'l'l

40

100

' I'l'l'l

100
J

10
10

10

f
i1

10

10

-=1 i

sz 10
"

-1

10

^i

p=-

\
c

^10

40

I ' I 'I'l'l

-Environment: 5M Kl +1000MV; 10
_ R.T.
I

10

^^

10

= I ' I 'I'l'l

-Environment: 5M Kl +500MV; ~^=J 10


R.T.

rs

(6 of 6)

Kmax (MPaVin)

(5 of 6>

Kmax (MPaVin)

T3

XI

10

10

I . I.I.I,
40

17.50 (min)
20.
25.
30.
34.00 (max)

RMS %
Error
37.84

XI
-1

10

-2

10

1 . 1,1,1,

10
4

100

10

40

100

Kmax (Ksivin)

Kmax (Ksivin)
Kmax (KsiVin)

io1 |

III I

10

JZ

~~

10

Li

1-

-2
10

10

. I I I III

10 2

"

o
"

10

10

10

"a
10

Kmax (KsiVin)

da/dt (10"3in/hour)

16.50 (min)
20.
25.
30.

1161.
18558.
25355.
36711.
66053.

32.50 (max)

RMS %
Error
>100.0

Figure 6.16.3.2.6 (Concluded)


6-424

da/dt (10"3in/hour)
503.
25954.
37810.
45074.
98475.

Ti-6Ai-4V
h
.V
M

CM
,'l^p.
cv
Q0
C5 *MC3* :-:-:-:^J7JS-:-:
Sw""' '"-Gff'
00
1X1
00

-:-:-:&::-:-:-^jft-:

w
5
0

mm IS

ssesjs

00
0

"S
as

Test
Time
(min)

HO

03
00

CM
tCS

<N

sss*:;
':...

:::::*:-:::

"<t*

S-
a*

r-l

^*;!

v::::+::::

t-

J>

1-4

1-1

>
^
t>

<

o>

o>

<R
M

^^ '.'.^^

-<*'
:*

<3>

MM

r-:

sso*;

WM

* ...

::: : ::
:S8Ki&': : : : >: :i : :

^s

^?
:-:-:-:jy-: :-x-:^^:-: ^?
CJl
eft S :--'!'3:-: 03
:.> CO
CD
a>

^
*
o*
SSSS

sip
;:iSi(i:: ^SS All SsMs
'Cy--

:>:::::>:

^^
*

r0
;S|Hg

re
0
0
OS
CO
*

t-

1-1

:t''

oc
?SB*s

cq
CO
CM

liip

CO

93

CO

e*
tr

(N
c03

t-H

1-1

^
cc

05
t~
OS

<N
t-.
<3)

i?s*?

1-1

JmaS?
S:K;

ssa*s

SS:.*:?

::::;: :::

:::::::

<N
CO
<N
*

:->::.:::::

:::::!::

**^

s^

+
CO

<!>

*g

C~

..

gSttg

t~

to

$$$&

fe

.r i

. *CO .
ta

+
OS

<0

t-

*^N

S
.*

Prod
Thk
(in)

e
2
u

CO
CO
CO

3
::;

: : :*:i::::

CO
CO

to

fie

tO
TH

05

&
00
0

CQ
55

lH

ta
r*

in

r-t

lH

:*o ::*a

;.'

tft

i-i

:::::::

AS

Kv:::?::::.

\o

>

T*.

**,

T-;

to
to

CQ

ssrSj's

u
lO

1-

to
lO

lp I

1 III

SSSSB

lO
:*&

:. -r':

*o

S*

ssjgs
J$

*
to

/to.

CO

S S

C -w

M
u

Test
Temp
(F)

* E
OH

ad
CM

oq
r-i

r-l

CO
i-3

H
J

11

ipl
a&
0)

-)

iO
O

1-1

to
to

0
p

"^

*o

iiii

g
l

H
J

*s *.

KrWi+A

5S1I

to

00

::'00

"* "^

00

10

to

:.1-f

>H

*<

PQ

iiiii m

,_!

A&iWtix-

111 z

u mm
a

ss^;:;

I
if

2
#
10

CO

10
CO

l>
to

CO

oi

lH

TH

l-C

0,02

to

!-(

TH-

:::::::;:;:*:::::
o:::*::<:

e^

P<

0
es

5S
to
CO

CO

-*

CO

*
1-H

CQ

CO

EH

1-H"

E^

E-1
C5

E-i
tf

CM

EL]

fe

3S

"2e *>a
0

to

*
::::::*:::

fri

s-s
0

bo

05

<g

1:

m m ;:

uS3
2

SSI*:* W::::*?; :S$:$-::: i;Sjp;S SSSiS:


.::::::.:-

be
,

ss^te

00
to
i

C4

iiiois

T-t

* ;***:

/ <r>

-*

OS

00

to

>::::]*::

to "!MO:
T-*

Ui
O

ao
*K*S

S*

i:&S|jf;

t
1

:::::::

OB

,N-"0

fa

o
CO
i-H

o 2 2 6
oH6S

X 0
rt c5 CO
5 >
fac3 .0
fH U
to
<N r
1-* j

to CO

Sor.u
lH fe

1-1

6-425

>-

Ti-6A1-4V
>V

00
b

CO

us

S3

00

OC

00

HQ

131

ssep
s&tgspe

<~

05

05
rH

:::::!::

iiao*

00

CM

(N mm
to

to
IO

OS

05
rH

C5

05
H

I
i

>:*:*x*:

<*>

sssos
4SCK:
t-f

IO
IO

05
<>
OS
rH

i
i
i

:::::!:::

eo

TJI
00

SSsrSS

rH
t05
rH

t-

SStH*
:;rH

i
t

:-:-:-:-:-x*>:

OS
(N
C-

OS

00

05
rH

00

05
rH

w%a%

t-

, c
ifflsos
05
r-l

i
i

00
ifcSO:':
SSOSs
r><

OS-

-re:

05
f*

i
i
i

f
i
f

; .

;..

00
00

'::*:*:::;

y^

*8
B

*
O

CO

<>

CN

<N

rH

to

tO
r-l

<N

to

IS

4
OS
05

+
05

IO

VH'

05

IO

CO
CO
Ttl

IB
*

05

to

03

to

<N
A

05
to

to

CO

**
05
U3

CO
111

^^Mi^SM

S^^^?^::^v::::

0 o
a B
A

P
Z

: i :w*$::

2-B.S

ri

eH

.2 3
a
S

till
*:*:*:*>:

J3

'
a,
as

a
as

:|:;:|:*:|::

i
i

B
H

IO
05

to
05

::?!:>:
V

;:: : : :t:i :::

'

tfxj;:!:

TO

CO

IP
wgjj*

n
rn ^J^
OH

to
05

to
t~l

I
t

to

::::-::+::

TO

to

to

CO

rH

rH

to

; TH

rH

rH

a
ffi

00

00

Hi

Hi

c
'B
o

ffifcS)*

0
CO

o
men

lit

ill e

n S: m
u
w

IO

&

ta

n '"O
m m

Hi

00

"

s
fa
1

to

CM

-5

mm

3 *,

05

05

r-l

rH

rH

rH

S
o
c

mm
o

11
lli

<5

as

:^:i-:-:iiS:
i

i
:<:<<:<::::*:''.:::

to
r-l

T-4

to

UV

<N
rH

d :

CO

<o

:::::::::

:W:'iy:-:;:

00

IP

10
05

>

::::::::

*>:>*::x;
00

HI

>

:*SSi:::::

: : ::

,00

i
i

:::::*::

rH

J
O

..'

lllpll::
$ S

rH

.
fa

CO

'

H
J

1 Sfe

E-i

E-i

tf

H r? w

IB

fa

fa

fa

cd

ft fa

"3 a

3*
I*
0 s

OB

2
to fa
a
rH O

rH

6-426

>
3

J.

iss4?:i;ii

F 1.5hr
1160F
1025 F
rAC

:::

1750 FWQ;
1000F 8hr
1000 F;

'

F 1.5hr
050 FF8hr;
F8hr

M
CO
50

1
1

:>:-::+:-::

^^
Q

MartinMarietta
Refined Grade
Hydrazine

3s

.- + ,C

t- >

rH r* 00

T1-6A1-4V!
a

00
00
CO
5
00

<fi

(3
w 9
OS +>
9

Test
Time
(min)

HQ

IB

Is
15

Prod
Thk
(in)

u2
Q
H

D
Z
c
o
S

0
S8SSSS
CO

CO
CO
5
CO
CO

eo

CO

05

03

t
:-::::+::

tCN

1
1
1

CO
rH

io

to

CO

3
CO

:::::+::-:
t

i
i

ID
CN
CN

to
CM
CN

I-H

iSsii

rH

<N

CN

Hi
*SSK

0
KSOS

00
CO
CO
CO
CO

fig;

CO
03

1
1

::-:::+::
i

eo

|;p8

CN

::::>::

<N

CO

eo
o

CO

eo
o

law-is
:::::+::

jljjl:

re

SS*?
::::-:::

CO
CO

CO

eo
o

CO

eo
o

CO
CO

eo

CO

CO

CO
CO

CO
00

00

CO

CO

CO

eo

00

CO

CO

CO

CO

CO

CN
l>
03

CN

CN

CN

CN

CN

CN

CN

CN

03

03

CM
l>
03

CN

03

03

03

03

03

OS

03

i
i
i

i
i

i
i

to

CO

+
CO

03
03

Ali

CN

eo

CO

CN

to

CO

C3

i
i

03

+
CO
03

CO
rH
rH

CO
rH
rH

CN
CN
rH

eo
o

rH

CM
03

rH

CO

CO

CO

eo

CO

CN

CN

03

CO

rH

rH

rH
iH

IO
rH

rH

rH

rH

CD
00

i-H

00

to

1
1

+
rH

CO
i
i

1
1

CN
00

1
1

C-

eo"

i
i

CO
rH

CO
03

r-i

CO

CO

CN
CN

<N

CO

CO

eo

eo

IO
y-i

U3
I>
O

IO

rH

US
1-H

iH

CO

CO

CN

CN

CN

CN

eo

CO

CO

CO

CO

oa

03
2

PQ
2

oa

ea
2

PQ
2

oa
2

IO

to

CN

J5
CN

;"><M

CN

EH

EH

a
as

eo
CO
5
i-H

*
e

SO

EH

1 I

>

CO

to

0)

Yield
Str
(Ksi)

CO

"0
o
E

hi 5

"a-s

1
OB

E
to

eo

3
'S
C
r-1

03

03

rH

CO
rH

503
#

e>
u
s

io
CO

*<

1-1

r-1

S *
an
CO w

Test
Temp
(F)

E
< IM
'S

EH

EH

E-i

EH

E-;

PS

OS

OS

fa

CM

OH

'S

03

0)

CD

ho

1
CO

QC
|M

"E ^

03

oa

6-427

ITi-6Al-4Vi
00

'S

*2$s:

o
o

r
o>
mm

t-

OS

o
o

o
o

05
00

OS
00

as

o
05
00

05
00

ft-"

OV

OS

05

00
: tp :
SSS

til

CO
A

OS
00

Ol
00

os

05

ssos:

mm

:: ov

HI
+
OP

mm

CO
A

00

mm

fin

iS-

ca

w
cc
ep

I?

o
e

in

HI
AHO'.-

in

10
CN

CN

;;;

fl::

is

l . :

to
id

la
id

tO;--

>*

in

CO

8
03 C
5

|
a,
o to

safer

C
CO

PH

ill

>

bo
C

&

pa

to
id

in

: ui i

a
as
a
a

EH

E-i
CO

CO
eo

3 n

in
CN

tt
E-<

EH
I

Sa) fa
o

EH
I

toI

EH

EH

PS

Ei

EH

EH

EH

EH

PS

PS

PS

PS

PS

fa

"a
o

1
o e

Ti ,C
CN

sfa
u
m o
U o

Hi

il

+ O
CO o

Di ^

I-l

T3

$u

T3

-Sfa
co
fa

55

6-428

IH

2 " -

sfa
w e
H JS S a

^ &fa

T3 5S
o>

'53 Ji c

.TU6A1-4V',
u

o to
o

00
00

w C

"ffl "a

Test
Time
(min)

HP

t
05
rH

i
i
I

m
<m&

xa

*>

$*i?

o*

MM.

:::::*::

00
CO

sss*;
ssfcSps

00

a* ::::*:
aafcws

t05
rH

i
i

rH

rH

CXI
CXI

C5

::**'

:v."-:-:-i-:-:

rH
00

1-1

SS*:;

rH
t~

:-:

t
Ol

o>

:;*

rH

:::::!:::

rH

exi
CM

rH
00
rH
t05
rH

i
i

rH

rH

1
:W*i*:
pCJP4
H

CXI
CM

rH
00
rH
t-

t-

en

rH

rH

i
i
i

4
:-:-:-:-:-x-:-;

iS
rH
wm

rH

<H

CXI
CXI

^
H

rH
00

3fH

T-*

t~

t~

ffil
.. 1*

00
TH

cr>

sstss
<33
rH

rH

>
1

rH

t>

I-H

CXI
CXI

?ii

rH
CO

mt)

CO
OS
O

t-

c- WV&ggii

rH
t05
rH

t-

r><

05
rH

i
i

:-::::::

co

<D
CO

::::-::+::

i
I

:::;::::::r::::

t~
iSSSSSK:::?

Eft
rH

:::-::::-::::::-:

3fi

00
CO

i
i

+
+

i
i
i

T
4

+
3

+
eo

'*

-rH
CO

+
00
CO

es

CO

CO
1

5
rH

**.

CO
CO

+
<>

to
igpittX^j

':^rH

00
00

W:*:*:*

i
i

-.:

:*:*:*:*:

!:!:!;!^:!:j;::

^-s

rfi

mm

+
00

:::::*:-:

4
4

1
1

:>:::*:-:

4
:-:-:-:-:-x-x
4

i
i

1
1
1

t
:-:::::::

1
1

JO

Prod
Thk
(in)

2-S
u

e
S

0
1-1

rH

2 s

exi

n,:
CM

39

CO
rH

S*

ffl

0.
CO

CO

to

rH

:::::!::

CO
rH

.
**

111;

exi

O*

CXI

CM

<N

CM

(N

CXI

".

CXI

CM

CM

'?

to

<*

o
u
lli
mm

iHl

PQ

co

tt

ffl

'

l A

<N

CXI

CXI

CM

exi

>

CXI

::::::-:

:-:::::::

m
a

C3

II
H

>

B 6 S'

ill 2co 35

rH

HI

II!
sl
BS
<D rH

ill

:::::::<:-

<x>
t

rH

<

:;:::v::::::::":::::::::::

<H'

*-

:*:::*::

i-t

4-

03

1::

111

I
z

CD

s
iil
Pie*

CO

ei

HH

lliiil

si

1
*

CO

B*

IO

T-t

rH

to

CO
fH

CXI

HJ

'H

: IO

to
eo

e^

Test
Temp
(F)

> 0
PH fe

:::;:::::::::::::*.:::::::::::

;::*::*::::::

IS
}
S:S:*S

c
OS

1
1

CD

s>J

:>:&*:*:
CO
rH

gg

<

::::::::

:::::::::;:.;:;::

.-.-.-.v.-......'...'

pS fa 'H
ffi *> .

00

so

I-:*:***:

S::!:::*?:
eo

CO
rH

;:::!:!:H:!:!;{

03

PH

Cii

CO
r
^a

"as
o s

OH

C
si

It!

<

i
6-429

Ti-6A1-4V
CD

co

o
o

3
Test
Time
(min)

CO

11

OS

PS

5s

co

CO

CO

e es

HO

CO

01
1-1

rH

CO
CO

CO

CO

CO

CO

CO

to
to

i-i

CO

>*

IO

CO

o
I
PS
CO

03
i-l

CO

If
m 11 11

CD
CO

CO

o>

CO
A

o
to

*:***:;::

as

t/5

C~

t-

as

SS Ss?>& Wt$S sgsag

_^

li

co

to

IPs

CD
CO

CD
38BQS
5 SjfOJ
k0

to

slaS*

CD

CD

CO

PS

PS

PS

PS

CD

CD

CO
t-

CO

CO

OJ

05

03

03

Ol

i-l

rH

iH

1-H

CD
CO

CD

sie*;:

i-l

to

to

mm
-t

tN

CD

CO

':
OS
to :j:g

CO
CO

co

to

eo

ll
n<

CO-

m icl
PS M 111

PS
CO
t-

o>

CO
t-

-co

03

OJ

IH

03
to

1-H

rH

S*S*::
03

:s:s*;:

lull
o

:
ASMS

,CO

to

mem

IscBl

CO

CO

CO

b-

SSS*S

:.,>

Prod
Thk
(in)

JS
'S
te C

1
1

1
1

::::>::
".>

to

IO

to

1-<

i-H

1-H

to
rH

9
*

to

to
to

to
to

MS

tfl

to
to

no

fQ

CQ

*Q
r*

:*::-:: :-:::::+::
T
T

MS

l&li

':;-

Ift

1
1

i
i
i

::::-::<-:-:

4
:-:-:-:vi-x

to

to

to

to

:i-t.

TH

1-H

-t

to
to

to

to
to

to
to

to
to

: J

ift

CQ

CQ

CQ

"'

co
Q

to
CM

to
(N

to
CM

to
CN

MS
MS

to
to

IO
to

IO
to

CQ

PQ

CQ
U
Q

CQ

T*'

JS
H

c
0!
S

:&:::::::::

J3 _

"P*

o
e
"0.
OS

MS
A

MS
MS

1ft

m
at

:&$

&
00

CO

o
P

f3Cf ijp

f
c0

St
T> -3 .5
jB^

i-i

-1

-(

E
c0

e
c

IN

Cu

*
0)

"ci a

a
a
C

1*
1

OB

6-430

mk P P

o5

<-J

CQ

CO

lil

NE-

CO

..:,;,:-?Asd.; :;;;-

IN
IN

EH

E-J
CiS

* 0

" S

U
P

TH

iH

E?
&

t-

Test
Temp
(F)

Ti-6Ai-4V
u

to

liipl

9
a

^M


00 **

Test
Time
(min)

HQ

:':;.

t""'.
SSSSSB;:*:

;*;:?*;;:;

SS8S*:S:

CD

CO

I-H

05

05

CO
tC3

CO
tOS

1-1

iH

O
00
OS
iH
CO

00
OS
1-1

CO

assail

CO

CO

::::

I*;:

I*

*-H

kH

05

05

05

05

CO
to
SS*?*: S:*;:

CD
t03

CO
tOS

CO
tOS

CO
t03

.-t

tt

1-1

1-1

1H

i-l

<s>

00
1-1

CN
03

CO

CO

CO
CO

CO

CO
CO

CO

t-

1-1

00

00
t-

CD

m $$
::**S%:

ssss

ssaas is;*;:
mem assess

to

-: :V'.0 '::

to

1-1

i~<

IS

CO

TO

JO

>o

o
o

lO

Prod
Thk
(in)

89
A
u

*
*-

00

wmm
:::::::>:<::::

00

'

CM

CM

lO

'

::::::::

i
i
i

CO

CO

+
CO
lO

to

1
1

'

1
1
1

*ffi?

to

m
: "^S : step
l|;
CO
WB
wm ;t:;
:

mmi OS
;;S Ji.S*l5

8005

ssso;:;

*;*#;:

OS

*a

l~

*o

U)

XvX-X-X- :':v:':-:':':-:

S g
o

WM
O)
SSBS
OS

;**<:;

to
id

. -MS'

id

td

to

111

lO

in
in

s';s;**;;;l

os

OS

CO
03

00
CM

:Wi*:K
i-l

to

CO

tn

mWm

-<*
lp;i

&
00
9

lllfll

a
(a
>
&

n
o m

lO

lO

to

id

id

>d

n m
m
o o

O
O

in
id

icQ

in
id

pp;i Ifl

fa *K

tf
9 fa

(S S^

"*o cs

<N 2
CN c
rH

c0
e

TH

J2

^1

OS

i-l

+
in
OS

tn

1
1

SSH&'SS

CD

Cd
: in

CM
CO

; o

.t-H

in
i-5

to

Ulli

C5
xn

TO

cQ

to

CD

CM

rH
1-1

mm

in s*os

E
J

ll|l

OH

iH
CO

o
Z.

{*

co

:::::::::

*s

I!

PH IP1

t-

Sii

eo

CD
P

t-

T-t

i-H

:4s;*#s;

iH

CD
OS

roo
oo
o

," >::::::::::::*:::::::

<N

to

liii
a;

00
t-

H>

::::5:

ta
to
ac

<N
in

ttW:*:':':':':':*

rH

to

S -v
2 S

fi

03
CO
OS

S '.?

; ':<* ;i;

to
m
in
00
c-

r-i
CO

i-MtS-

CO

iH

CO

i-

EH

CQ

EH

^ c

fa c

BH

KSSSsJSS

HH
02

03

OH

i
i
i

O
CS

to

to
:. .:--r<
CO
:

i-H

eo

z,

o ffi:-?**::::
z. 111

in

eo
eo

CO

04

00

eo

eo*

EH

in
00

to
CO

E-i

fa

fa

05

&< fa
"5 a
O

fa

1
OK

sa)
+

73 ^3

0)
N

Is

S^S fa

E-i fa
-

0 9

O >n
JO

6-431

fc

a> is

T3

"u
a
m
C

! Ti-6A1^4V j
o

;*:;
':<=>

SE

cs

00

'::'0.

mm

SOS:
CD

CO

HP

if;

so

o>

0)

ja;

HI

T*

S&S SSOj
:H.
Hi

:,:!
SOS

i't-

*; n

spSi

IS

3
Wii SSS*
SHK;

2 c
o

0
p

:*S:

so

m
;

a
ft
as

-a

Jf *J

#1

aa

tN

05

p*

0)

Ieo

p*

-s

to

00

CO

OS

fa

fc

ce
0
o

PN

0)

"5
o a

I*
d
oS a
US

o
a)

ce

c
a
E

P4

ft

ce

a
a>
SO
f-t

a
co

o
o

is

ce
A
*
ce
a

ce
o
p*

CO

S fife

OS

a
S
EH

g h
ftQ

o
es
ft

CO

6-432

0)

ce

SO

ft

Ti.6Al.4V ELI

J
CO

"8
4*
V

tQ

fl

0
+*
l0

-tu

1o-

O
fi

eo

CO

oo

CO

CO

eo

" &
tea

f-H

0 *

0)

,w

bf

g*

CD

a
en

H
i

es
W
M

i-l

CO
t-

CO

lO
CO
00

C3
V

u
H
w
es

<

<

IN

o
O

'
o S

fa fa

o
a

&

60
C

T?o

fc

PH

6-433

Ti-6A1-4VELI

ise*

*-*

SSOS

O
H

1-3

**s*s^;?.

iiipi

CM

CM
CO
CO
CM

CM
CO

CO

CM
CM

CO
CM

CM

CM

es

CM

-91

CO
(M

iisiii

MSiKSSSSK

KSSSSHWSSS

am

ft*

CO
CO

CM

CM

CM
H

Z II
%m$m

02

fa?
02 CU

CM

o"

Z
0
D4

1^

gS

H2

00

CO

03
CO

CO
CD

CO

CO
CO

CO
CO

E-i
<>

g<?

S3

H
J

llillll

flk

O
2

Cd

cu

S
Q0

u.
sSss

HP!

11

H
<
H

Z
H
h-1

Z : i??*
SS*-*
i^a
SI1I 1111*
OS

P3

CONDI
HEATTRI

o
o

ca

mmmm

z
ez

&
>

i-4 1
-5
53
X!
o
us

02

03
02

o
W8i

<

III

6-434

00

CO

Ti-6A1-4V ELI

CM

SO:

swHy

*3.

e *

IS:

ii
mm

&
1*3!

<y^

is
CO

6-435

H-6A1-4V ELI

CM

o
o

<

Ol

50
00
CO
CO

WMi

co
cq

/-*l

p-4

CO

t-

to
CO

CO

63

$3&SSS*8

iiiiii

ill
mgtm&

:**s*3;s::?s?

mmm

CB
OQ

as

o
*a

fa

fa

*3

tf

Cfi
fa

O fa
GO OH

9~N

fa

fa

lO

fa

1-4

sO

fa

Q
fa

l|pSitll

CO

i&:*k:-

fa
>

op
Sfa

%
WSBi

CU

ill

Ck

N3

O
HH
H
<
H

fa

1-4

tf

::Z

:*:*:*:::;
-

r
lApB
: : ."

:
mil
JsSs*Sssis*# *:****
::::;:::
:

H3

CONDI
HEAT TRI

CP

-H

::::::::

<
ffl

111

6-436

a
o

U3

Ti-6A1-4V ELI

9
o

:**!*v:::

41

m
3!

t-H

CO

w
H

;.:.:'::

Si

ii

HI

CO

02

BD
O
CO

"*
N

a.

Sa

N3

o
o

PQ

>

CD

Z
O

>*

6-437

T1-6A1-4V ELI

et*

#;$

::::

:*:**:

Si*

s*

:^:::::-iiiwv>:>:::::^

ft

::-:-:::::.*(:::

d
l(

-*
V)

llllli lift!
8 iiliii

IIII

IQ

r~

*Q

U3

:J

Z
W

Z
0

*
C*

tf

?
c4

tf~

to

**

~*

CO
'::-..

fX^^
K

liiiii

oP
:g
faT

CU

&

O
HH
H

<

HH

xllS
SSSS

::$:&:

SrW

SI11I
lpiiii
s:J?*iiasjj^s?
<

ca

OH

Hl

w
HI

6-438

Ti-6A1-4VELI

o
<s

>:

O
H

1C

fa

5
Q

ez

CO

Z
fa

3D

z
o

O fa

fa

fa

3w

.5

tu

3
iiipi

fa

c-

CO

-1

00

'.**

tf

CO

<y~
S

O
O

U3

*""1

o"

U3

Iplllll

fa
>

Bs

s
D-

CO

CO

i$?3;

fa
CD

o
o

CO

/-V

CO

CO
CO

00

: fk.;

o
p

<

-z, :.
H

fa

op

-* fa

<

03

iftillll
O

CH

6-439

~*

~*

CO

Ti-6A1-4V ELI

>::::
-<

O
H
O

o
o

iiiii
3 lllllsl
liilll
X!

CO

03

zB

fa

03
CO

fa
ti

fa

H
co

2
o

O)

w
<s
v
N

c-

r-

00
U3

t-

cs

CO
CO

ifpll
>

is!;
:g88S8*i>*S

3
iiiii
:l$;

ft!

lilll
p
iiiii!

IG

ti

fa

O fa

fa

CO

c~

CM

fa
fa

CO

fa

O
O

>;^\ ./

llilll

fa

z
5

o
fc.

II

CD

J
H

ililiiiii

ta

o
H

H
<J
H

z
fa

l-H

:-.z 111
^*(s -*-* *
s

*:$S

1111
filfllli
i#II!l

S:?::

H'l

**">'

Q3
ZH
iplllll

:-:-:-:-:::::::

Illi

D
W

2
;:;*.*

<

Ulli

6-440

;Ti-eAl-4V EU I

O
H
O

fa

o
o

to

Z
fa
H
Z

CO

cc

fa
H
cc
fa

O fa
cq

CO

ja

fa

CO

fa

O
O

111

SI
IHII!

fa
>
I

i'ggfa

CD
N3

El

mm

Z
O

zfa
3
o

6-441

T1-6A1-4V ELI

o
JA:

<

O
H

;g:ja;

fat
1 HI
iilii

CO

to
N

cs

00

""'

:-:-:-:-:-:-.*.*^fc>:-:

lllSp|:|

CO

o
va

fc

05

Ulli

CO

lllll

CO
fa

<u
mm
*

CO

o
ti

t^

o-

cy~

CO DH

I-*

w
CO

3O
Q O

to

[',;V

t-i

c**

5>

g^
3
CO

12

Ss
og
22

F*^

&

':S:*:*:-

11!

O
HH
H
<
H

zH
N*

$i?S:

**;*;*

S
iSipiiii
t^mzmmi

III

. Z
wmmmm

<

ca

6-442

Ti-6A1-4V ELI

IS*!'!'*::

O
H

O
O

^f

k
CO

II

cc

BB

EM

o
i-H
i-H
SO

^
**

&

ABBAS*!"

1
3

Ilil
-fe,.

CO

to

to

cy
J3 N

lO

^r-:

ft

*d

64

O
O

o>

id

O
cc

fell
mmm

fc

/-S

tlllSI
cc itfiil
o
^

cc

o>

N
00

~*

e-t

CO

:: :

: : :Q5::::IW::::::::::::::::::::::

O
H

<

Z
H
HH

^.-Zvv
HS
lilgilli
ipiiii
mjtmmtmm

SSSS

<
a

6-443

Ti-fiAUV ELI

8
z

I
2>
t/s

I1-*
z
o

C4

CO

o
w
&
00

Bo

ill
J

5?g

Pisfc
P

8a,

<

O
U

z
z

<

ES
>
as
o

6-444

T1-6A1-4V ELI

I
feS
if.

rfl
2s*

d
i

rf
OS

ei

in

go
So
w

i*

IB

gig
E

PS

si

z
<

Cd

o
a

a.

o
Si

Si

6-445

z
z
<

I Ti-6AI-4V ELI h
Condition/Ht: ANNEALED
Form: 3 in. Forging
Specimen Type: CT
Orientation: LT
Frequency: 1 - 10 Hz
Environment: LAB AIR; RT

Yield Strength: 116.8 ksi


Ult. Strength: 126.7 ksi
Specimen Thk: 0.991 - 1.014 in.
Specimen Width: 7.4 in.
Ref: NC002
(1 of 1)

AK (MPaVin)
4

10

AK (MPaVin)
4

40
100
i I i I i|>l

- I

10

i I >|i|i|

40

100

' | M'l'l

10
-2

10

10
_aj
o

10

<o

" 10~ 2
o

'I

6^10-4

Z. 10

~ 10~
^-^

"<3

=
p

_fi t
10

z
~ 10 \
u
x>
-

10

10
4

10

40

da/dN (10"6in/cycle)

16.
20.

25.
30.
35.
40.
50.
60.
67.30 (max)

Life Prediction Ratio Summary


an
0.

40

10

100

da/dN (10'6in/cycle)

AK (KsiVin)

2.29
2.44
6.73
13.3
22.2
35.9
58.1
91.3
210.
487.
1039.

12.87 (min)

13.

RMS %
Error
5.04

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , I,I,I,

" I , I,I,I,

100

10

r~

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


I-'

0.

Figure 6.17.3.1.1
6-446

.5

.8

1.25

2.

H Ti-6AI-4V ELI r
Condition/Ht: ANNEALED
Form: 3 in. Forging
Specimen Type: CT
Orientation: TL
Stress Ratio: 0.1
Environment: LAB AIR; RT

Yield Strength: 116.9 ksi


Ult. Strength: 127 ksi
Specimen Thk: 0.999 - 1.002 in.
Specimen Width: 7.4 in.
Ref: NC002
(1 of 2)

AK (MPaVin)
1

10
-1

= i ' i 'i'i'ir

40
100
1 | I I Mil

ID

(2 of 2)

AK (MPaVin)
4

I- I

10

40

' I 'I'I'II

100

' I 'I'I'I

10

Frequency: 10. Hz

10

u
\
10

10

10

10

10

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

40

0.700
0.903
3.15
8.34
17.3
28.7
44.3
67.1
159.
408.
567.

35.
40.
50.
60.
63.28 (max)

RMS %
Error
12.15

Life Prediction Ratio Summary


o
I

0.

.5

.8

100

da/dN (10"6in/cycle)

AK (KsiVin)
12.55 (min)
13.
16.
20.
25.
30.

5.71
6.57
12.2
22.1
33.4
51.4
85.8
249.
377.

15.12 (min)
16.
20.
25.
30.
35.
40.
50.
53.22 (max)

10

AK (KsiVin)

AK (KsiVin)

1.25

RMS %
Error
4.28

Figure 6.17.3.1.2
6-447

Life Prediction Ratio Summary


a
0.

.5

.8

1.25

2.

\ Ti-6AI-4V ELI
Condition/Ht: BA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: TL
Stress Ratio: 0.
Frequency: 15 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(1 of 5)

K (MPaVin)
4

- I

10

' I M'l'l

40

' I 'l'l'l

Environment: Dry Air; R.T.


10

= I

10

40
1

' I M'l'l

100

I M'l'l

Environment: Water Saturated -=q 10


_
JP-4 Jet Fuel; R.T.

100

(2 of 5)

AK (MPaVin)

10

10
2
io" ^

"

_Q)
O

frl 0"+
\
c
_
z: 10
o

,0-1

10

_K I

10

-5

10

10

10

10

- i , i,i.i,
4

i , i,i,i,

10

40

100

da/dN (10"6in/cycie)

AK (KsiVin)

RMS %
Error
21.95

12.8
17.6

24.9

.8

100

da/dN (ICTMn/cycle)
0.315
1.12

5.09
12.8
22.9
32.4

50.1
56.2

43.49 (max)

36.1

.5

AK (KsiVin)
16.
20.
25.
30.
35.
40.

Life Prediction Ratio Summary


0.

40

14.45 (min)

0.110
0.217
0.934
4.47

11.53 (min)
13.
16.
20.
25.
30.
35.
37.95 (max)

10

AK (KsiVin)

AK (KsiVin)

1.25

RMS %
Error
12.01

Figure 6.17.3.1.3
6-448

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

i Ti-6AI-4V ELI h
Condition/Ht: BA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: TL
Stress Ratio: 0.
Frequency: 15 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(3 of 5)

AK (MPaVin)
4

10

c=iI I I I'!'

40
-II

100

10

40

100

I 11 llll

Environment: Distilled Water;


R.T.

-2

(4 of 5)

AK (MPaVin)

10

Environment: 3.5s NaCI; R.T. -= 10

10

10

10

10

io-3

-3

10

10"2^
o

o 10
-3 Jz

10

-5

-o

o
o 10
\
c

io" ^
o
\

10

-3 |

Z 10

10

L."0

10

_.iT3

10

XI

T3

10

10
10

10

10

10

10

10
.-8

10

10
4

10

40

100

da/dN (10"6in/cycle)

RMS %
Error
20.50

100

0.227
1.34
4.02
11.3
29.9

10.07 (min)
13.

1.24

16.
20.

5.45
12.2
23.0
38.5

24.47 (max)

51.4
51.9

Life Prediction Ratio Summary


-1

0.

40

da/dN (10*6in/cycle)

AK (KsiVin)

0.959

15.4-7 (min)
16.
20.
25.
30.
35.
40.
40.10 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i , i.i.i,

- i , i.i.i,

.5

r-

.8

1.25

RMS %
Error

Life Prediction Ratio Summary

26.12

Figure 6.17.3.1.3 (Continued)


6-449

.5

.8

1.25

2.

-\ -6AI-4V ELI h
Condition/Ht: BA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: T-L
Stress Ratio: 0.
Frequency: 15 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(5 of 5)

AK (MPaVin)
4

10

i ' i M'l'i

40
T

AK (MPaVin)
1

100

= I

1 I I HIM

r ,

10

40

' I 'I'l'lI

100

' I 'I'l'l

10

Environment: S.T.W.; R.T


-2

10

10

10

10

10
10

-2

10

JR

io

o
frio-4

10

\
io

10_JE
10

10
10

-^"0

10

-o
10

10

-5

10

10
-7

10

10

10

10
10

'

I I llll

10

10

I I I 111

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


0.

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.399
1.54
3.23

13.53 (min)
16.
16.98 (max)

RMS %
Error
4.83

10

AK (KsiVin)

AK (KsiVin)

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary

i-'

2.

0.

Figure 6.17.3.1.3 (Concluded)


6-450

.5

.8

1.25

2.

I T;
Condition/Ht: BA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: T-L
Stress Ratio: 0.1
Frequency: 1 Hz

- I

10

' I M'l'l

(1 of 6)

40

' I 'I'l'l

(2 of 6)

AK (MPaVin)
1

100
_L
0

io"2

ID"2

10

- I I n't

40

100

I ' I 'i'l'l

-1

Environment: Water Saturated


_ JP-4 Jet Fuel: R.T.

10

Environment: Dry Air; R.T.

10

10

io-3
QJ

5^10-

io~

Ja

^^-

Z10"5

10

>
x>

_3E

10

rJr

-^

E
*^-

WE

-z.

Z10"5
-o
\
o
~

WT

io"2

jf

6-10-4

, E

10_3E

<D

o
\

10

io"3

<u
m

10

-1

-1

\
D
"

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140

AK (MPaVin)
1

-6AI-4V EL.1I I1

10

>
"O

"6
10
-5

-5

10

10

io"7

10"7
-6

-6

10

10

io"8 "

I , I ,l,l,
4

I , I, I,!,

10

1C)0

.40

" 1 , 1,1,1,

io-8

6
da/dN (10 ~ in/cycle)

RMS %
Error
3.90

,40

100

Life Prediction Rati<3 Summary


i

0.

.5

.8

1.25

6
da/dN (10 " in/cycle)

AK (KsiVin)
27.33 (min)
30.
35.
40.
50.
60.
70.
72.48 (max)

61 2
131
221
407
414

40.32 (min)
50.
60.
70.
71.02 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , I,I,I,

2.

RMS %
Error
8.12

Figure 6.17.3.1.4
6-451

22.4
25.1
40.1
60.8
104
203
399
571

Life Prediction Ratio Summary


0.

.5

.8

1.25

2.

^ Ti-6AI-4V ELI
Condition/Ht: BA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: TL
Stress Ratio: 0.1
Frequency: 1 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(3 of 6)

AK (MPaVin)
4

10

- I ' I Tl'l

10

40
100
I I Mill

Environment: Alternate JP-4


Jet Fuel & Distilled Water;
R.T.

10

- I ' I Tl'l
-=i
-

(4 of 6)

AK (MPaVin)
40

100

1 ' I Tl'l

Environment: Distilled Water;


_
R.T.

10

-d

10
10

10
-3

10

10

iio-2 ^

o
\
-3|
10 E

o
+

fri o-

10

10

10
10
X>

10

.-6

10

10

10

10
-7

10

10

10

10

10

' i i i in

10

i 11 n

40

10

'

i i 11 ii

100

da/dN (1(T6in/cycle)

AK (KsiVin)

I ''''

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

63.1
141.
210.
383.
607.

42.57 (min)
50.
60.
70.
74.51 (max)

19.2
31.1
48.9
69.0

26.24 (min)
30.
35.
40.
50.
60.
70.
73.62 (max)

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
1 2.68

122.

212.
388.
489.

Life Prediction Ratio Summary


i

0.

.5

r-

.8

1.25

2.

RMS %
Error
6.05

Life Prediction Ratio Summary

Figure 6.17.3.1.4 (Continued)


6-452

.5

.8

1.25

-I TJ-6AI-4V ELI
Condition/Ht: BA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: TL
Stress Ratio: 0.1
Frequency: 1 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(5 of 6)

AK (MPaVin)
4
10
i I i Mill

40

100

' I 'I'll

Environment: 3.5s? NaCI; R.T.

(6 of 6)

AK (MPaVin)
4

= I

10

40

' I 'I'l'lI

100

' I 'I'll

- Environment: S.T.W.; R.T.

-=\ 10

-2

-=J 10

10

10

-1

10

10

10

10

io~2

io" "
O

6-10-4

frlcT4

-3 EI

10"JE
10
10
o

10
10

.x
a

10

T3

10

10

10

10
10

10

10

10
10

'

I I ilMl
4
10

Li

i i 11 ii

40

10

100

da/dN (I0"6in/cycle)

AK (KsiVin)

107.
138.

214.
365.
628.
1018.

.5 .8

1.25

2.

RMS %
Error
10.25

35.5
55.2
69.5
87.7
217.

620.
754.

Life Prediction Ratio Summary


0.

Figure 6.17.3.1.4 (Concluded)


6-453

100

da/dN (10-6in/cycle)

27.01 (min)
30.
35.
40.
50.
60.
64.60 (max)

Life Prediction Ratio Summary

0.

10
40
AK (KsiVin)

AK (KsiVin)

53.1
73.9

26.53 (min)
30.
35.
40.
50.
60.
70.
73.43 (max)

I I I I III

I II III

AK (KsiVin)

RMS %
Error
6.28

.-6

.5

.8

1.25

^ Ti-6AI-4V ELI
Condition/Ht: BA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: T-L
Stress Ratio: 0.1
Frequency: 0.1 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(1 of 2)

AK (MPaVin)
1

4
10
40
100
Ti I i I'M!
i ' i ' Ml'
Environment: Water Saturated
_
JP-4 Jet Fuel; R.T.

10

I I I 'I'd

I-

40

100

I ' I M'l'l

10

-= 10

10
-3

10

10

_aj
u

6^10-+

6^10\
~~
c
_

10-E
10

-^

z
X

, 10
10

10
-7

10

10

10

10
'

'

i i i i ii

10

10

I i I i li

40

- i ,

I,I,L
4

100

da/dN (10~6in/cycle)

AK (KsiVin)

118.
244.
459.
1199.

.5

.8

100

13.8
33.9

26.86 (min)
30.
35.
40.
50.

103.
209.

369.
551.
1627.
2758.

60.
70.
75.41 (max)

Life Prediction Ratio Summary


0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

15.9
27.4
48.2
69.5

26.50 (min)
30.
35.
40.
50.
60.
70.
76.78 (max)

1 , 1,1,1,

10

AK (KsiVin)

AK (KsiVin)

RMS S
Error
9.50

3E

10 ^
o

XI

-6
10

ill

XI

2
10"

10"

-Z. 10

10

10

-1

Environment: 3.5s8 NaCI; R.T. 10

10

10

o
~

(2 of 2)

AK (MPaVin)

1.25

RMS %
Error
17.62

Figure 6.17.3.1.5
6-454

Life Prediction Ratio Summary


I--

0.

.5

.8

1.25

2.

This page intentionally left blank

6-455

^ T1-6AI4V ELI
Condition/Ht: BA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: T-L
Stress Ratio: 0.5
Frequency: 0.1 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(1 of 4)

AK (MPaVin)
4

10

40

100

= I
Environment: Dry Air; R.T.

(2 of 4)

AK (MPaVin)
10

40
I

' I 'I'l'l

100

I I Ml'!

Environment: Water Saturated 10


_
JP-4 Jet Fuel; R.T.

10

10

10

10

-3

10

10

o
_
6^10-4

fri oc

2
10
o
\

10"

10"JE

_
/

10
-o

_K

10

10

10 \
u

\
o

"O

-6 -

10

10

10

10

10

10

10
10

I , M,l,

- i , i,i,i,
4

10

40

'

10

100

.5

.8

100

da/dN (10-6in/cycle)

AK (KsiVin)

3.34
6.89
13.7
24.5
44.6
76.9
101.

35.

37.10 (max)

Life Prediction Ratio Summary


0.

40

14.08 (min)
16.
20.
25.
30.

4.58
5.96
11.6
22.4
33.4
55.8
57.9

14.31 (min)
16.
20.
25.
30.
35.
36.37 (max)

10

i ' 11 ii

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

'

i i 11 n

AK (KsiVin)

RMS %
Error
8.04

^^

-z.

10

1.25

RMS %
Error
8.44

Figure 6.17.3.1.6
6-456

Life Prediction Ratio Summary


r~

0.

.5

.8

1.25

^ T1-6AI-4V ELI r
Condition/Ht: BA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: TL
Stress Ratio: 0.5
Frequency: 0.1 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(3 of 4)

AK (MPaVin)
4
10
f=-i> i i I'M
i-

- Environment: 3.5s NaCI; R.T.

40
100
II I 1 MIH

(4 of 4)

AK (MPaVin)
10

40

100

I ' I 'I'l'l

- I ' I 'I'l'l

31

Environment: S.T.W.; R.T.

10

10

10

10

10
10

10

o
o 10

6^10-4

-3 |

-3 |

10

10

10

10

_i/0

10

10

10

10

10
10

10

10

10

LL

i' iin

' i i i HI
4
10

10

40

i I i I Hi
4
10

10

100

da/dN (I0"6in/cycle)

35.28 (max)

RMS %
Error
15.51

0.

.5

.8

1.25

4.60
5.38
12.9
26.5
53.2
116.
217.
395.

15.38 (min)
16.
20.
25.
30.
35.
40.
42.70 (max)

Life Prediction Ratio Summary


i

100

da/dN (10"6in/cycle)

AK (KsiVin)

6.43
6.87
17.2
34.1
203.
294.
305.

15.54 (min)
16.
20.
25.
30.
35.

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I I.I.I

i-'

2.

RMS %
Error
7.85

Life Prediction Ratio Summary


i

0.

Figure 6.17.3.1.6 (Concluded)


6-457

.5

.8

1.25

i--

2.

^ Ti-6AI-4V ELI r
Condition/Ht: BA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: T-L
Stress Ratio: 0.5
Frequency: 1 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(1 of 6)

AK (MPaVin)
4

- I

10

' I M'l'l

40
T

100

= I

I I MIM

10

' I M'l'l

40
100
i I l I MM

Environment: Water Saturated -=\


_
JP-4 Jet Fuel; R.T.

10

Environment: Dry Air; R.T.

(2 of 6)

AK (MPaVin)

10

10

o
\
10

10

10

10

10

40

100

RMS %
Error
20.54

25.
30.
35.
40.

51.8
68.9
97.4
102.

41.26 (max)

Life Prediction Ratio Summary


.5

.8

1.25

100

0.592
2.27
6.61
13.5
23.7
41.8
67.4
113.
136.

10.91 (min)
13.
16.
20.

0.370
2.57
5.94
11.9
28.3

10.10 (min)
13.
16.
20.
25.
30.
35.
40.
40.48 (max)

40

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (10-6in/cycle)

AK (KsiVin)

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error
22.56

Figure 6.17.3.1.7
6-458

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

TI-6AI-4V ELI r
Condition/Ht: BA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: T-L
Stress Ratio: 0.5
Frequency: 1 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(3 of 6)

AK (MPaVin)
1

4
1

10

I I I MH

Environment: Alternate JP-4


Jet Fuel & Distilled Water;
R.T.

10

40
100
i I i Ml

40

10.34 (min)
13.
16.
20.
25.
30.
35.
36.59 (max)

RMS S
Error

22.73

40

100

I ' I Tl'l

Environment: Distilled Water;


_ R.T.

10

100

10

40

1^

100

AK (KsiVin)

da/dN (10"6in/cycle)

.5 .8 US"

da/dN (10"6in/cycle)

AK (KsiVin)

0.208
0.247
2.16
5.72
13.0
27.7
42.1
58.5
95.3
173.

9.85 (min)
10.
13.
16.
20.
25.
30.
35.
40.
44.21 (max)

0.502
2.19
5.87
12.9
23.5
35.5
50.1
55.4

Life Prediction Ratio Summary


0.

10

-IM 'I'l'l

AK (KsiVin)
AK (KsiVin)

(4 of 6)

AK (MPaVin)

i-'

2.

RMS %
Error
16.37

Life Prediction Ratio Summary


1

0.

Figure 6.17.3.1.7 (Continued)


6-459

.5

.8

1.25

2.

^ TI-6AI-4V ELI h
Condition/Ht: BA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: TL
Stress Ratio: 0.5
Frequency: 1 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(5 of 6)

AK (MPaVin)
4

10

40

c=-1r-TT

10

100
rrmj-

- Environment: 3.5s NaCI; R.T.

40

100

16.
20.
25.
30.
35.
40.
40.69 (max)

RMS %
Error
18.26

.5

.8

1.25

1 ' I Tl'l

10

40

ZL
10

100

da/dN (10"6 in/cycle)

AK (KsiVin)

1.16
1.24
3.56
10.1
28.3
57.8
88.7
128.
190.
232.

9.76 (min)
10.
13.
16.
20.
25.
30.
35.
40.
42.18 (max)

Life Prediction Ratio Summary


0.

100

AK (KsiVin)

0.986
2.59
9.25
32.5
67.8
111.
194.
290.
300.

13.

40

Environment: S.T.W.; R.T.

10

da/dN (10"6in/cycle)

10.16 (min)

10

t I ' I 'I'l'l

AK (KsiVin)
AK (KsiVin)

(6 of 6)

AK (MPaVin)

2.

RMS %
Error
18.87

Life Prediction Ratio Summary


r

0.

Figure 6.17.3.1.7 (Concluded)


6-460

.5

.8

1.25

i--

2.

This page intentionally left blank

6-461

1 H-6AI-4V ELI
Condition/Ht: BA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: TL
Stress Ratio: 0.5
Frequency: 1 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(1 of 4)

AK (MPaVin)
4-

= I

10

40

'I 'I'l'l

100

' I 'I'l'l

"'

10

JF

10

<D

6-10-4

10"

-7

10

~~

"

I , I,I,I,
4

10
10
10
10

10

, I,I,I.

10

40

10
4

100

da/dN (10"6in/cycle)

0.

.5

.8

100

1.25

3.40
5.35
13.1
24.2
37.0
54.6
82.7
101.

14.71 (min)
16.
20.

25.
30.
35.
40.
42.28 (max)

Life Prediction Ratio Summary


i

40

da/dN (10"6in/cycle)

AK (KsiVin)

4.53
5.63
12.4
20.0
34.6
56.7
78.4
92.9

15.15 (min)
16.
20.
25.
30.
35.
40.
40.96 (max)

RMS %
Error
9.01

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

^-^

<"
10 \

4
z

10

10

10

2
10" o
o
\

10

10

jjp

-=j

10

rf

-o

100

' I 'I'l'l

10

10

40

10

fri 0"

10

' I 'I'l'l

Environment: JP-4 Jet Fuel;


175T

10

_L

Environment: Dry Air; 175T

(2 of 4)

AK (MPaVin)

i-'

2.

RMS %
Error
15.33

Figure 6.17.3.1.8
6-462

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

^ Ti-6AI-4V ELI h
Condition/Ht: BA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: TL
Stress Ratio: 0.5
Frequency: 1 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(3 of 4)

AK (MPaVin)
4

10

40

' I 'I'l'l

100

' I 'I'l'l

Environment: Distilled Water;


175T

(4 of 4)

AK (MPaVin)
4

- I

10

I I 'I'l'l

40

100

I I 'I'l'l

-i

Environment: 3.5ss NaCI; 175T 10

~d 1

10

10
10

10

10

10~

IQ"3

JE?

_aj
(j

^10"

io"JE

-r: 10"

Z 10

10
10

10

I
z

b-10-4
\
c
_

a>

m" ^
u
x>

_c

10

10

10

10

10

-= 10

10

I Ml

10

10

10.-6

i i 1111

40

da/dN (10"6in/cycle)

RMS %
Error
5.93

.5

.8

100

1.25

5.51
6.93
17.8
48.6
100.
159.
165.

15.01 (min)
16.
20.
25.
30.
35.
35.56 (max)

Life Prediction Ratio Summary


0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

20.2
28.9
52.4
71.2
93.3
104.

21.49 (min)
25.
30.
35.
40.
41.36 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , I,I,I,

- i , i,i,i.

100

2.

RMS %
Error
11.42

Life Prediction Ratio Summary


0.

Figure 6.17.3.1.8 (Concluded)


6-463

.5

.8

1.25

H TJ-6AI-4V ELI r
Condition/Ht: BA
Form: 1 in. Plate
Specimen Type: DCB
Orientation: T-L
Stress Ratio: 0.8
Frequency: 1 Hz

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 88140
(1 of 2)

AK (MPaVin)
1

(2 of 2)

AK (MPaVin)
4

10

40
100
-ii I i I i|i|
i- I ' I M'l'l
.
.
10
Environment: Dry Air; R.T

- I

10

' I M'l'l

40

100

' I M'l'l

Environment: 3.5s NaCI

-2

10

10

-Jio"2

o
o 10

fri o-

10

f-

10

-Z. 10

10

10

-o

XI

10

_R ~
10

-EL

sP

10

10

10

10

10
10

'

111in
LAA

'

10

.-8

10

1111ii

40

100

I I I I III
4
10

da/dN (1CT6in/cycle)

AK (KsiVin)

I . l.l.l.
40

100

AK (KsiVin)

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

0.187
0.328
0.594
1.08
4.63
5.09

7.50 (min)
8.
9.
10.
13.
13.61 (max)

RMS 55
Error

10

Life Prediction Ratio Summary


i

9.34

10

10

10

10

10

10

-a

.5

.8

RMS %
Error

1.25

Life Prediction Ratio Summary


0.

2.

Figure 6.17.3.1.9
6-464

.5

.8

1.25

I--

2.

Ti-6AI-4V ELI h
Condition/Ht: RA
Form: 3 in. Plate
Specimen Type: CT
Orientation: L-T
Stress Ratio: 0.1
Frequency: 1 10 Hz

Yield Strength: 119.4 ksi


Ult. Strength: 127.8 ksi
Specimen Thk: 1.003 - 1.04 in.
Specimen Width: 7.4 in.
Ref: NC002
(1 of 2)

AK (MPaVin)
4

- I

10

40

' I M'l'l

100

' I 'l'l'l

-1

10

t I ' I 'I'l'l

10

Environment: Lab Air; R.T.

(2 of 2)

AK (MPaVin)
40

100

1 ' I M'l'l

Environment: S.S.W.; R.T.

-d 10

10

10

-1

10

-3

10

10

5^10"+
\
c
_

Z. 10
-a

10"J E

tr

"o

o^10-4

_
.-6

10

Z 10
a

-Jio
>

10
10

10

10
10
10

i , I,I,I,

- i , 1,1,1,
4

10

40

10
4

100

da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error
45.17

.5

.8

100

1.25

3.61
3.78
7.01
16.7
32.1
57.4
120.
223.
372.
385.

10.88 (min)
13.
16.
20.
25.
30.
35.
40.
50.
50.76 (max)

Life Prediction Ratio Summary


o

0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.809
0.847
4.28
11.5
20.4
30.6
48.2
85.8
248.

12.94 (min)
13.
16.
20.
25.
30.
35.
40.
47.16 (max)

10

AK (KsiVin)

AK (KsiVin)

2.

RMS %
Error
20.08

Figure 6.17.3.1.10
6-465

Life Prediction Ratio Summary


0.

.5

.8

1.25

2.

^ Ti-6AI-4V ELI h
Condition/Ht: RA
Form: 3 in. Plate
Specimen Type: CT
Orientation: TL
Stress Ratio: 0.1
Frequency: 1 10 Hz

Yield Strength: 122 ksi


Ult. Strength: 130.2 ksi
Specimen Thk: 0.923 - 1.01 in.
Specimen Width: 7.4 in.
Ref: NC002
(1 of 2)

AK (MPaVin)
1

b I

10

40

' I 'I'l'l

(2 of 2)

AK (MPaVin)
1

100

= I

' I 'I'l'l

10

40

' I 'I'l'l

100

' I 'I'l'l

-Environment: S.S.W.; R.T.

-=j 10

-2

10

10
-3

10

<D

2
10~
o
\

o
6^10-4

10~

I
**
-z.

.-5

Z 10
-o

"
10 \
u

T3

10
10

10
10
.-8

10
4

10

40

100

AK (KsiVin)
da/dN (10_6in/cycle)

AK (KsiVin)
16.
20.
25.
30.
35.
40.
50.
60.
67.29 (max)

RMS S
Error
15.63

0.

-r~

.5

.8

i-'

1.25

100

3.07
3.70
8.22
20.0
44.4
91.9
134.
309.

13.17 (min)
16.
20.
25.
30.
35.
40.
45.43 (max)

Life Prediction Ratio Summary


A
o
-I-

40

da/dN (10"6 in/cycle)

AK (KsiVin)

1.53
1.74
3.67
7.61
15.8
30.1
53.6
89.9
228.
618.
1541.

12.57 (min)
13.

10

AK (KsiVin)

2.

RMS %
Error
31.46

Figure 6.17.3.1.11
6-466

Life Prediction Ratio Summary


o m
r

I-

0.

.5

.8

1.25

\ TJ-6AI-4V ELI h
Condition/Ht: RA
Form: 0.5 in. Plate
Specimen Type: CCP (max load specified)
Orientation: LT
Frequency: 8 Hz
Environment: LAB AIR; RT

10

40

Yield Strength:
Ult. Strength:
Specimen T-hk: 0.246 - 0.252 in.
Specimen Width: 3.995 - 4.005 in
Ref: NC005

(1 of 5)

AK (MPaVin)

(2 of 5)

AK (MPaVin)
1

100

10

40

- I i I i|i|>|
10

Stress Ratio: -1.

100

| i | TM

Stress Ratio: -0.66

10

10

10

10
10

10
o
o 10

.2?
o

o 10
c

10 \
O

Jj

10

-o

10

10

-=Jio
>

_K I
10

10

10
10

10

S
-6

10

10
10

I , LI,I,

I , I,I,I,
4

10

40

10

100

da/dN (10"6in/cycle)

RMS %
Error
10.56

-r-

.5

.8

100

0.201
0.208
0.547
1.11
1.92
2.97
7.40
11.7
22.0
33.5

5.97 (min)
6.
7.
8.
9.
10.
13.
16.
20.
21.02 (max)

Life Prediction Ratio Summary


a o
0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.219
0.234
0.591
1.30
2.19
3.10
8.07
18.3

5.92 (min)
6.
7.
8.
9.
10.
13.
14.97 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I , LLL

- I , l.l.l,

1.25

RMS %
Error
27.47

Figure 6.17.3.1.12
6-467

Life Prediction Ratio Summary


r-

0.

r-

.5

.8

1.25

2.

H Ti-6AI-4V ELI
Condition/Ht: RA
Form: 0.5 in. Plate
Specimen Type: CCP (max load specified)
Orientation: L-T
Frequency: 8 Hz
Environment: LAB AIR; RT
(3 of 5)

AK (MPaVin)
4
10
40 100

=. I i I Ti'l

Yield Strength:
Ult. Strength:
Specimen Thk: 0.246 - 0.252 in.
Specimen Width: 3.995 - 4.005 in
Ref: NC005

AK (MPaVin)
1
4
10
40 100
- I ' I M'l'l
1 ' I M'l'l
Stress Ratio: 0.

-1

I ' I M'l'l

10

Stress Ratio: -0.33


-2
10

(4 of 5)

10

10
10

10

_Q)

io"

10

10
-2 -7Z

10"
o

_0J

o^lO"4

6^10-4
c
_

,o-I

io
z 10

10

-10'\
o

x>

-6

10

10

"~~

10

10
10

10

10

"

1 , 1.1,1,

1 , 1,1,1,

40

10

10

10

da/dN (10"6in/cycle)

RMS %
Error
13.75

0.113
0.127
0.232
0.465
0.904

5.71 (min)

6.
7.
8.
9.
10.
13.
16.
20.
22.72 (max)

6.90
9.76
21.4
27.6

Life Prediction Ratio Summary


im
""I-

.8

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.114
0.137
0.294
0.662
1.38
2.50

5.68 (min)
6.
7.
8.
9.
10.
13.
16.
20.
20.90 (max)

I I 11 ll

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'

I I I I III
4
10

10

100

1.25

RMS %
Error
2.12

Life Prediction Ratio Summary


0.

Figure 6.17.3.1.12 (Continued)


6-468

1.61
4.71
8.71
21.5
33.5

.5

.8

1.25

-I Ti-6AI-4V ELI h
Condition/Ht: RA
Form: 0.5 in. Plate
Specimen Type: CCP (max load specified)
Orientation: LT
Frequency: 8 Hz
Environment: LAB AIR; RT

4
-

10

40

| l|>|'|

'

Yield Strength:
Ult. Strength:
Specimen Thk: 0.246 - 0.252 in.
Specimen Width: 3.995 - 4.005 in
Ref: NC005

(5 of 5)

AK (MPaVin)

AK (MPaVin)
4

100

| 'l'l'l

-L

-2

40
100
ni Minn
10

10

10

10

10
_a>

-2
o

frl 0"+
"~~
c
_

10

-J10~2

10

10

_,

.-6
10

-J10 >

Jio
>

10

10

10
10

10
10

10

o
o 10

10

"c

>II

10

10

-3

10

FT

10

Stress Ratio: 0.55

IAI.I.I,
4

10

i 1 11111

10

40

10

'

100

da/dN (10"6in/cycle)

0.0692
0.201
0.537
1.19
2.12
3.26
5.22
30.9
33.9

5.
6.
7.
8.
9.
10.
13.
13.28 (max)

Life Prediction Ratio Summary


i

0.

da/dN (10"6in/cycle)

AK (KsiVin)

0.0132
0.0150
0.0238
0.0402

2.34 (min)
2.5
3.
3.5
4.

RMS %
Error
11.19

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i i 11 in
40
100

i i 11 n

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary

0.

2.

Figure 6.17.3.1.12 (Concluded)


6-469

.5

.8

1.25

2.

^ Ti-6AI-4V ELI h
Condition/Ht: RA
Form: 0.5 in. Plate
Specimen Type: CCP (max load specified)
Orientation: L-T
Frequency: 10 Hz
Environment: LAB AIR; RT
(1 of 4)

AK (MPaVin)
4

_ I

10

i I i j' t':

40

Yield Strength:
Ult. Strength:
Specimen Thk: 0.249 - 0.254 in.
Specimen Width: 3.996 - 4.002 in
Ref: NC005

~=

-2

10

10

40

100

I. ' I 'I'l'l
I- I ' I 'I'l'l
- Stress Ratio: -0.66

Stress Ratio: -1.


10

100

' 1 'I'l'l

(2 of 4)

AK (MPaVin)

=l
10

10

10

10
10

io"2

o
5*10"+
c
_

o 10

-3 |

10

10

,-s

z: 10

z. 10
10

_fi -

10

\
D
XI

X)

10

10

-5

10

10
-7

10

Ill I

10

10

10

I , l,l,l,

10
4

10

40

'

10

100

da/dN (10_6in/cycle)

RMS %
Error
6.23

13.
16.
20.
24.13 (max)

ES

0.

.5

r-

.8

HI

100

4.11
5.83
10.2
24.0
78.1

11.44 (min)

Life Prediction Ratio Summary


i

i i i

40

da/dN (10"6in/cycle)

AK (KsiVin)

3.76
5.71
9.95
23.3
76.7

10.90 (min)
13.
16.
20.
23.96 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'

i ' i in

1.25

RMS %
Error
3.94

Figure 6.17.3.1.13
6-470

Life Prediction Ratio Summary

0.

.5

1-i

.8

1.25

2.

H TJ-6AI-4V ELI
Condition/Ht: RA
Form: 0.5 in. Plate
Specimen Type: CCP (max load specified)
Orientation: L-T
Frequency: 10 Hz
Environment: LAB AIR; RT

10

40
"Ii

' I 'I'll

Yield Strength:
Ult. Strength:
Specimen Thk: 0.249 - 0.254 in.
Specimen Width: 3.996 - 4.002 in
Ref: NC005

(3 of 4)

AK (MPaVin)

(4 of 4)

AK (MPaVin)
1

100

4
\=Ii

I ' I 'Ml

10

40

100

I i |i|i|

10

Stress Ratio: 0
10

10
-3

10

^10"4

_
-5

10
T3

"O

_.

-Jio >
XI

10
10
10
10
i

10

' i i i HI

i ' ' i

10

40

100

AK (KsiVin)
da/dN (I0"6in/cycle)

AK (KsiVin)

RMS %
Error
5.19

i-

.5

.8

100

1.25

0.249
0.230
0.280
0.488
0.931
1.71
5.25
8.32
18.6
69.6

5.70 (min)
6.
7.
8.
9.
10.
13.
16.
20.
24.00 (max)

Life Prediction Ratio Summary


0.

40

da/dN (10"6in/cycle)

AK (KsiVin)

3.73
5.50
8.98
20.3
82.1

11.07 (min)
13.
16.
20.
24.82 (max)

10

AK (KsiVin)

RMS %
Error
13.21

Life Prediction Ratio Summary


o a
i

0.

Figure 6.17.3.1.13 (Concluded)


6-471

.5

.8

1.25

2.

Ti,6Al-4VELI
0
o
C

CO

t-

3
w

0
CO

05

Test
Time
(min)

o a
HP

ll

t
i

+
00

Prod
Crack
Thk
(in)
(in)

I-H

CO
CO

-S e

l-H

d
0

CO

1-H

to

OS

&
8
o
Q

IB

t9
s
2

>
CO

Yield
Str
(Ksi)

BC

s Sfe

IB
fa fa

a.

ft
n
*>

X
n

to
0

e
S

fi

p*

0
0

a9

0
C

PS

a
a
C
0

i-l

03

0
o
a
(B
B

US

M
00

CD

o s
OS

.2

'S

u
o
toft

to

m
U
0
*J
OB

ee

6-472

Ti-6Al-6V-2Sn

!
.

,
'

t-

(
'

'

,
1

'

to Q

a ^
J! Sri

CO

CO

Tf

CO

CN
to

ao

i-H

CM

o
+J

1^
^
^
^
o-

0)

c J
o

AJ

fcf

B >

C
(9

J2

CM

CO

T-t

'

PJ

H
H3
CO

-0
>e

d
w

<D

-w
c

fH

'

co

eo

eo

<*

CN

CN

tCM

t-

CO

CM
CN

en
co

CO

oo
o

CO
tN
IO

f-H

00
CM

73

*-<

1Q

-j

o
o
o

OS

<

t~
lO

co

OS
Et, 50

o
<

OS

PS

PS

PS

B
fa

<

<

t-4

fa

Cd

Ja

Ed o*

cy

OS

PS

<*

Of

PS

a
IS
6
fa
o

X
O

*
<
o

CO

CO

<

at

ato

Eh
O

1-*

<

aco

<

HO"

Ed
pa

CO

IO

to

t~

it

<
o2

oo

fa
10

<

03
CN
*

CO
t-H

IN

T*

eo

*-t

fa
o

r-t

co

03

to a
C
(9 2
M

ra

CD

a.
en
c

CO

<
PS

PH

6-473

fa

<
O

00
c

OS

-M
01

cy

**

Ec
o
o
c-

Ed
pa

s
gs
u fc

fa

+J

Ti-6Al-6V-2Sn

*-t

s>
o
/s

8
^1

O
es

nisi

tiiii

TO

1
III

mtmuam

till!!
w&t&m

il
\j

mmm
0
tf

w
o

:;::

: : : *""t:::;k^3:::::::::::r:::::::::.

FH

CO
CO

*-4

?;:;:'-

iiiiiii
B
1I1II

3a.

I^lgilli
&^
CO
iJ

&

o
M

H
H

<

HH

tf

;&::;$

111
H

^H

5
Sil
S"< SJ :

?:?:?
::*:*:*
:

&

Hs -

<
IG

III

6-474

Ti-6Al-6V-2Sn

mm

O
H

o
o

a??;::;

S;is**s;i**i:s:

fa

<

ts iiili
o

CO

1-1

fa

02
02
fa
fa
ti
H D

cc

oc

l>

s
is*
S3?*::

OS

3
assesses
>

<1
O
X!

CO

fa

fa

fa

ff-.
fa N

CO

cd

l-H

to
fa

J-Si

tf

aQ O
fa

Z
ii
fa
fa

d
Q CO

fr*

fa

BS

Og
CO

0.

.-fc:

o
H

H
H
Z

<
fa

S
o

H
Z

&w

||ipll
Miiiii

lM;Sfaf;$8*

<
to

ZH
fa

6-475

Ti-6Al-6V-2Sn

o
o
^-<
o
o
o
/*".

11

00

05

:::::::::+:::::-::

to

Z
H

':

ft*

8fc,

05

to

a?

:*0'

Z
O
tf

0*^

~*

CM

CO
iH

i'^'*

.'

IPIIII
Bg

iiilll
H

liiiii
lSilll
A :

a.
S

i-9
*

14
O
NH
H
<
H
Z

NH

tf

is;S*
: : : : :: : :

Z:

: : :: : : :

888

NH

5 $&&.
laiiiiii
t"< -3
<3

CONDI
HEAT TRE

::x:;::x;:

ssssi

<
to

111

6-476

n--6l-6y-2Sn

o
SS:;
*m

o
o

<s

.8

0
W)

02

I(

CB

S3
C 5

Z
W

Z
O

PH

lill

liilli
iiiii

8
Illl

0?~

,5

00

SO

o
Ho

i<

W
es
Q CG

1
B
1

iiilliiii

O
Z
o

fV:

14
O
H
<
H
Z
W
pH
PH

PH

.:':"-Z.
H

og

mm&m%&

H,i

CONDI
HEAT TUE

PQ

tf

mm*~m

pH

1
llllp!::;:
::::::::+.::::

<

6-477

I Ti-6A1.6V-2Sii

ssos
:S*?

Q
H

o
o

a?;:

/-s

00

*tf
CO

.32

<

X
X

gZ

fa

to
CO

fa fa

e PH

z
o

C")

CO

CO

t>

Ill Si*:

lilS!

S::S!Ss?ili

IliilpSi

liplf

11111 *;s
II1
llli

OS

fa

O
iq

fa

fa

to PL.

?
CO

fa

&*

Is

fa

*"*

fa

s os

fa

*H

hH

fa
fa

ipiii 111

fi
Q CO

IN

fa V

H
J

P lllf
IPPIII WM
iliiili iii;
1*11
SB*:**

z
o

H
<

Z
fa
hH

NH

HS;**'

*;;

III

%%
;*!*!**'
pilll
::::::::
fc"< Z*
:::::::

ZH

<
P
r*
CO

::::::::

6-478

Ti-6Al-6V-2Sn!

o
o

;:;:
>:?lr^:

30K

c*>

3
PC

CVS

ipii

**

as

H
Z

8
a mtm

to

'mmm

V3

z
0
ti

w
&*>

Pill

CO

06

l-H

CO

o
d

:v: ;.,:-;

&*
2
O

35
3

Il!i
H

05

Z
O
M
H
<
H
Z
H
HH
(1
O

H
z

iH

illltl
og
** 5

iSSlfcii

ZH

<
2

111

6-479

Ti-6Al-6V-2Sn

SOK

;:**;:

****:
/T-s

111

ffliSl
Z

o
^ :::::;:S:;:S:*ij::;:::
CO

llftil

TICS

C3

&mf&msg

*>

z
o

JO
'S

tf

o
o

WgSgiljgl;::

3
fltt

cy^
Htt

*-H

o'

EJ

0.

a,

rH
CO
1-1

to

IPIIIII
Bs

I
SI

op

CO
I

..g-.fe ;
JV

o
t1
H
<
H
55
W
h-(

SKSI
::::.::::

H
Z

^rW

5s
lillll
msi^mm^m

*:;:&::;:
SS-SS:

<
CO

<
CO

ZH
ffi

HI

6-480

Ti-6Al-6V-2Sn

5S
O
H
U

o
o

JO
*".

<

CO

15

fa

CG
CO

D
CO

O fa

z
o

.5

fa

00
00

P3

00

o
1

ti
*3

fa

C?^

S N

p5

3o
Q

;>& ..,.

fa

Z
NH

1-1

fa
fa

CO

Bg

a
0.

:: :

: : :fiSft:WW:::::::;:;:*::::::::::

CO

O
hH
H
<
H
Z
fa

h*

tf

A*

H
Z

SSSS
iW
iZisilll

ipill
'f^%m&mm *>:*>:*:
H-5S-

CONDI
HEAT TRE

CO

00

iiii

CO

lH

ao

00

mw*~m

CO

CO

ISP ISIS*:o

<
to

||1

6-481

Ti-6l-6^2Sn:

Si-OS
*:*!?:

O
O
/*>

IM

US
CO

es

II3I11

Hill

filltll

00
*

TO
C-i

Iliil
j;i:ss*3i*:gs?

Z Iii
H

o
o

S
Z
o
pel

es

<y~
N

JVJ

_H

CO

1
&

'

a.

25

W
D

J
Ei
14
O
HH
H
<
H
Z
h1

Ck

H
Z

Ipllil

pill
t* >

<

is
ZH
OH

6-482

Ti-6Al-6V-2Sn

o
r-<

o
o

*;**

ti

saos

<
fa

ii

co

cq
^

/s

.33

<

fc

00

r-

to

TO

50

tlgll

:::::::-:-+*:::

lltpll

si*;*;**:::*

mm

W
H

ii

TO

ilili

TO

CO

HS

*s otf
I5
few
o@
o
F-t

^
3 N

CO OH

3s

CD

;:A

DEFI
SnAT

H2

<
W w

ffl

iO

&

H N

53CD

fa

1-H

CO

liil^ll

flC "F*^ -- -

A''.:

-V

O
M
H
<
H

iH

H
hH

'" 5*

Z:

s
OS

<
CO

lilplll
fa

6-483

Ti-6Al-6V-2Sn

CM

<

O
H

ti mm

"w

CD

i<.>

i-3

im
0

Mi
1

n
mm

S3

llll
1-1

00

EKj

so

a
w

SS
Pfii

K
Pu
03

w
CO

O
O

< I?
J3

e
sc

6-484

Ti-6Al-6V-2Sn

IS!

is
<?

.31

iH

0*

00
CO

IS
pi

Ed

SSI

6-485

Ti-6Al-6V-2Sn

es

n
M

til

^ EC -

oz

0
GO

CO*

si?
zi*

tu
CO

f-

id

A.

IB

4*
o

gig

E-

e e -

BJ

Bi

Bi

B!

a
a
o
Z
o

3
is

?B

6. fe

*E

2*

Eh

CD ix

6-486

**

Ti-6Al-6V-2Sn

3
!

5>

is
g

jag
3^

z
g

H
Z
O

M
Q

CO

ii*
H
9gi

is
H
oi

Bi

si

&

O K

2
O

!3
IK

H 3
Z

ill
iE '

6-487

S E o 8.is

5 * *" o < -.

&. o sa

Somg <fa

Z*-

u fc

3
a

a u

si

s
n

nfufi X

S3gg
tn
6. o

fc

S3a 3

es

3>
5

J;

tf

8
S

rfau

3 a 1~

Q
H
ii

H
Z
O

CD

CO
H

So

cd

B*

CO

i*

9*5

6-

BB -

B~
o

6
S
gg-

<

5 o 2 5 5 fe
(as 25 <S

Irs

^ Q* ft*

g io io g
pa

< a.
E=8
U 00
S3 -

6-488

Ti-6Al-6V-2Sn

I
is
tf

(<fi

*a8

\ii*
z
2X

d
CO

i
CM
CO

O .
Jl Of

B?.

CO

H
PQ

S3

9si

as
9

H B

8;" o

ts&c

si

BS

ft

Hi

a?

as

i
8

a 2 <

S3 oS

30K-

SMI

CD

ft

S B S
m P O S

iBB

8|

go
S H ta

63

r w. s

6-489

S8
d

RS5

! Ti6Al-6V-2Sn |

I
41

*lt
3 J

II
E
O

as
a
H

EH

id
15 =
CO
CD

i>

9g?
H

&
E*
K

cd

erf

J
E-

E-

E-

'S

s
as
o

Q
W

<2

<

6-490

ar

3S
< a,

i-3 J

PS <

8 fa

Ti-6Al-6V-2Sn

I
tf

^P

ftf
a HS
Q
H

Z
l-H

gli<
z
S
M

O
U

Sir
CO
11

i*

to

H
9|
a

h O

1 "

si

1*

ill
a

SHU

Of

or

%,

Is
log

Of

OS

6.

s &

fa >

6,

fc.

* '

g'
6-491

2S
<"
o

28
o

i"z

Ti-6AI-6V-2Sn

I
5>

is
rfS

*a8

Q
W
Q

it*
z|<

as

X
M

f>

CO

S do

00

ii*
3|
Kg
feO

6
o

Of

Of

Of

Of

1=

6> -

I*
S

8
-4S

68
<S
o

6-492

This page intentionally left blank

6-493

EF

Ti-6AI-6V-2Sn h
Condition/Ht: BA
Form: 0.38 in. Plate
Specimen Type: PTSF (max stress specified)
Orientation: T-S
Stress Ratio: 0.1

AK (MPaVin)
4

10

' ' 'I'l

(2 of 3)

AK (MPaVin)

3)

40
100
i I U UM

11

Yield Strength: 130 - 160 ksi


Ult. Strength: 168 ksi
Specimen Thk: 0.375 in.
Specimen Width: 5 in.
Ref: 90981

= I

10

40

' I M'l'l

100

' I M'l'l

Environment: 3.5 NaCI; R.T.;


_
Frequency: 10. Hz

-Environment: 3.5 NaCI; R.T.; 10


Frequency: 0.1 Hz
10

10

-1

10

10
-3

10

10

_0J

_0J

I io-2

2 TZ

10"
6^10-'

o^10-

-3|
10 E

-3 |

10

-z. 10

10"

10

-S

10~

10
-5

10

10

10

10"

10

10

10

i in'
40
100

i i'l
4
10

LL'

10
4

16.9

Life Prediction Ratio Summary


i

0.

100

1.01
1.07
1.94
7.24
16.6

8.91 (min)
9.
10.
13.
16.
17.02 (max)

RMS %
Error

1111ii

40

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (10_6in/cycle)

AK (KsiVin)

10

AK (KsiVin)

AK (KsiVin)

16.37

10

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary

i-'

0.

2.

Figure 6.18.3.1.1
6-494

.5

.8

1.25

Ti-6AI-6V-2Sn f
Condition/Ht: BA
Form: 0.38 in. Plate
Specimen Type: PTSF (max stress specified)
Orientation: TS
Stress Ratio: 0.1

10

- I ' I 'I'll

40

Yield Strength: 130 - 160 ksi


Ult. Strength: 168 ksi
Specimen Thk: 0.375 in.
Specimen Width: 5 in.
Ref: 90981

(3 of 3)

AK (MPaVin)

AK (MPaVin)
4

100

1 ' 1 'ITI

Environment: H.H.A.; R.T.;


_ Frequency: 10. Hz

= I

10

' I 'I'l'l

40

100

' I 'I'l'l

10

10

10

10

-3

10

10

io"

io'2^

^10"4

o
o 10

o
\

-3 |

10

10

Z10

10

_Jio
>

XI

.-6

XI

10

-*-o
10
o
x>

10

10

10

10

10

10

10
10

EF

~ I I.I.I.
4

I , I,I,I,

10

40

10
4

100

da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error

Life Prediction Ratio Summary


i

0.

.8

40

100

1.25

RMS %
Error

Life Prediction Ratio Summary


0.

2.

Figure 6.18.3.1.1 (Concluded)


6-495

da/dN (10"6in/cycle)

AK (KsiVin)

i-'

.5

10

AK (KsiVin)

AK (KsiVin)

.5

.8

1.25

I-1

2.

^ Ti-6AI-6V-2Sn
Condition/Ht: MA
Form: Extrusion
Specimen Type: CCP (max load specified)
Orientation: LT
Stress Ratio: 0.02
Environment: LAB AIR; RT
(1 of 2)

AK (MPaVin)
1

10

40

Yield Strength: 143 ksi


Ult. Strength: 157 ksi
Specimen Thk: 0.081 - 0.082 in.
Specimen Width: 3.509 - 3.519 in
Ref: MA002

100

10

- I i I Tl'l

i I i 11 Ml

- I ' I 'IT

(2 of 2)

AK (MPaVin)
40

100

I ' I Tl'l

Frequency: 20. Hz

Frequency: 10. Hz

10
10
-3

10

io"2^
o

10

10

u 10

Z 10
X!

_. :

~o

10

10

-7

10

10
10
4

10

40

da/dN (10"6in/cycle)

RMS SB
Error
4.86

0.

.5

.8

100

1.25

0.0182
0.0464
0.0988
0.174
0.279
0.431
0.653
2.22
5.10
10.4

4.16 (min)
5.
6.
7.
8.
9.
10.
13.
16.
18.61 (max)

Life Prediction Ratio Summary


i

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.130
0.130
0.178
0.271
0.426
1.51
3.77
8.00
15.9
30.9
61.9
128.
168.

6.99 (min)
7.
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
41.81 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I I, III.

~ I , *l,l,

100

RMS %
Error
5.05

Figure 6.18.3.1.2
6-496

Life Prediction Ratio Summary


,

0.

.5

.8

1.25

2.

-i Ti-6AI-6V-2Sn h
Condition/Ht: MA
Form: 2 in. Forging
Specimen Type: DCB
Orientation: L-T
Stress Ratio: 0.02
Frequency: 0.1 Hz

Yield Strength: 144 ksi


Ult. Strength: 151 ksi
Specimen Thk: 0.75 in.
Specimen Width: 5.5 in.
Ref: 84360
(1 of 2)

AK (MPaVin)
1

(2 of 2)

AK (MPaVin)
1

4
10
40
100
- I I I 'l'll
I ' I 'I'l'l
-L
10
Environment: Dry Air; R.T.

tr I

10

' I 'I'l'l

40

100

' I 'I'l'l

Environment: Dry Argon; R.T.

10

10

JZL

10

10

""

.32
o

o^10-+
\
"*
c
|_

J2
o

o
\

u 10

-3 |

10

ZIG"5

10

10

Z 10
10

10

~o

10

_K
10
10

10
10

10

10

10
10

10

10

10

-3

"

I , I,I,I,

I , I,I,I,

40

10

10

'

RMS %
Error

da/dN (10"6in/cycle)

0.

.5

.8

i 11in

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


i

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'

i i 11 n

100

RMS s
Error

Life Prediction Ratio Summary


i

.5

1.25

Figure 6.18.3.1.3
6-497

.8

1.25

i Ti-6AI-6V-2Sn h
Condition/Ht: MA
Form: 2 in. Forging
Specimen Type: DCB
Orientation: LT
Stress Ratio: 0.02
Frequency: 1 Hz

Yield Strength: 144 - 155 ksi


Ult. Strength: 151 - 164 ksi
Specimen Thk: 0.75 in.
Specimen Width: 5.5 in.
Ref: 84360
(1 of 4)

AK (MPaVin)
4

10

40

(2 of 4)

AK (MPaVin)
4
10
"II I I 11)!)

100
_L

40
100
11 I I 11111

Environment: Dry Air; R.T.

10
-1

10

-3

10

"""

10"2 "

10
\
c

10

Z 10

-Jio
\

XI

10
-5

10
-=i

10
10
10

I , LI,I,

" I , Mil.
4

10

40

100

AK (KsiVin)
da/dN (10"6in/cycle)

AK (KsiVin)

10

40

da/dN (10"6in/cycle)

AK (KsiVin)

4.81
6.34
10.00
17.7
30.0
48.9
87.2
674.
923.

13.02 (min)
16.
20.
25.
30.
35.
40.
50.
54.97 (max)

RMS %
Error

Life Prediction Ratio Summary


,

0.

.5

.8

100

AK (KsiVin)

1.25

2.

RMS %
Error
17.35

Figure 6.18.3.1.4
6-498

Life Prediction Ratio Summary


i

.5

.8

1.25

Ti-6AI-6V-2Sn r
Condition/Ht: MA
Form: 2 in. Forging
Specimen Type: DCB
Orientation: L-T
Stress Ratio: 0.02
Frequency: 1 Hz

Yield Strength: 144 - 155 ksi


Ult. Strength: 151 - 164 ksi
Specimen Thk: 0.75 in.
Specimen Width: 5.5 in.
Ref: 84360
(3 of 4)

AK (MPaVin)

(4 of 4)

AK (MPaVin)
4

4
10
40
100
i | i | i|'|
1i I i I 'IM
Environment: JP-4 Jet Fuel; ~=\ 1
R.T.

10

40

' I M'l'l

100

' I 'I'l'l

Environment: Distilled Water;


|_ R.T.
10

10

10

10
-3

10

10

-Mo~
o

o
^10"4

a
-3 |

10

10

o
o 10

|_

2 10

10

J2

io"2^

\
10

10

10
10

10

10

10

10

10
.-8

10

i I i I Hi

10

40

I I I I III

100

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


i

0.

.5

40

100

RMS %
Error

Life Prediction Ratio Summary


0.

1.25

Figure 6.18.3.1.4 (Concluded)


6-499

da/dN (10"6in/cycle)

AK (KsiVin)

r-

.8

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error

10

10

10

.5

.8

1.25

1 Ti-6AI-6V-2Sn
Condition/Ht: MA
Form: 2 in. Forging
Specimen Type: DCB
Orientation: L-T
Stress Ratio: 0.02
Frequency: 10 Hz

Yield Strength: 144 - 155 ksi


Ult. Strength: 151 - 164 ksi
Specimen Thk: 0.75 in.
Specimen Width: 5.5 in.
Ref: 84360
(1 of 4)

AK (MPaVin)
4

10

40
Ii

TTTI

100

I i M|i|

\- I

=q

10

40

100

i I i | i|i|

' I ' I'M

Environment: Dry Argon; R.T.

10

Environment: Dry Air; R.T.

(2 of 4)

AK (MPaVin)

-1

10

10
-3

10

10

.2

o
&10"+

^io~2

6-10-4

_D-

-3 |

10

-s

10

__

"o

"a

10

10

Z 10

_R

10

-5

-=|l0 >

13

10

10

10
10

10
-7

-7

10

10

10

10
10

'

I ' III!

10

10

I i I i It

40

'

100

0.

.5

.8

I ' I 'I'

40

100

da/dN (10-6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


r~

10

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

'

i ' "ii

AK (KsiVin)

RMS %
Error

RMS %
Error

Life Prediction Ratio Summary


r-

0.

1.25

Figure 6.18.3.1.5
6-500

.5

1 TI"

i-'

2.

\ Ti-6AI-6V-2Sn h
Condition/Ht: MA
Form: 2 in. Forging
Specimen Type: DCB
Orientation: L-T
Stress Ratio: 0.02
Frequency: 10 Hz

Yield Strength: 144 - 155 ksi


Ult. Strength: 151 - 164 ksi
Specimen Thk: 0.75 in.
Specimen Width: 5.5 in.
Ref: 84360
(3 of 4)

AK (MPaVin)
4

10

40

100

Environment: JP-4 Jet Fuel;


R.T.

- I

' I 'I'l'l

- I ' I 'I'l'l

T=J

(4 of 4)

AK (MPaVin)
10

40

' I 'I'l'l

100

' I 'I'l'l

Environment: Distilled Water;


R.T.

10
10

10

10

10

10

10

-B-

-ET

o
^10"+

10

io~
o
\

o
^10"4

10

_c

10

-o

X>

10

10"2^

"ET

10 ^E

_
10

-5

z:

-a-

Jl0 >

-*
10

ii-

10

10
10

10

-6

10

10
.-8

10

10

' Mill!

i I i I ill
4
10

40

.5

.8

1.25

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


0.

10

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

1A

i i Min
40
100

' i i 11 n

100

AK (KsiVin)

RMS 55
Error

-=10

RMS ss
Error

Life Prediction Ratio Summary


i

0.

2.

Figure 6.18.3.1.5 (Concluded)


6-501

.5

.8

1.25

i Tl-6AI-6V-2Sn h
Condition/Ht: MA
Form:
Specimen Type:
Orientation:
Stress Ratio:
Frequency:

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 91945
(1 of 1)

AK (MPaVin)
40

AK (MPaVin)
4

100

Environment: Interstitial Oxygerr= 10


_ 0.16; R.T.
-

40

100
10

10

10

10

10

10

IQ"3

_0J

_qj

10

*-"*

"O

_R I
10

10"

Jio
>

^-^

-z.

z 10

QJ

10~ o
>>
o
\

-5

"O

o
o 10

10

m~ ^
u

10

"

10

10
10

III I

10

10

I III I-

10

I III

10

10

i , i.i.i,

10
4

10

40

10.-8

100

I , LI,I,

I , I,I,I,

40

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


i

0.

100

da/dN (10"6in/cycle)

AK (KsiVin)

7.83
12.2
31.4
62.8
124.

18.53 (min)
20.
25.
30.
31.63 (max)

RMS %
Error
12.00

10

AK (KsiVin)

AK (KsiVin)

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


i

i-'

0.

2.

Figure 6.18.3.1.6
6-502

.5 .8

1.25

-I Ti-6AI-6V-2Sn r
Condition/Ht: RA
Form:
Specimen Type:
Orientation:
Stress Ratio:
Frequency:

Yield Strength:
Ult. Strength:
Specimen Thk:
Specimen Width:
Ref: 91945
(1 of 2)

AK (MPaVin)
4

1
___

10

| M 111

(2 of 2)

AK (MPaVin)
1

40
100
-1I I I Mill

= I

Environment: Interstitial Oxygens 10


_
0.08s; R.T.

-2

10

' I TIM

40

100

' I 'I'PI=R

Environment: Interstitial Oxygerrs: 10


_
0.16; R.T.
^

10

10

10
-3

10

10

v
10

o 10

o 10
c

10

10

Z 10
o

-Jio \

\
o
O

-6

10

10

-5

10
10

10

10
i

10

10
4

10

40

100

I i LLL
lMI
4
10

da/dN (10~6in/cycle)

35.
40.
50.
60.
70.

10.9
23.7
47.1
71.6
97.7
116.

35.
40.
45.04 (max)

177.

80.

195.
197.

90.
91.66 (max)

RMS %
Error
11.34

da/dN (10"6in/cycle)

AK (KsiVin)
21.24 (min)
25.
30.

4.48
6.34
13.7
22.8
34.1
49.0
87.9
124.
151.

18.44 (min)
20.
25.
30.

100

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

II

40

Life Prediction Ratio Summary


i-'

0.

.5

.8

1.25

2.

RMS %
Error
6.60

Figure 6.18.3.1.7
6-503

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

i Ti-6AI-6V-2Sn h
EF
Condition/Ht: STOA
Form: 0.63 in. Plate
Specimen Type: CT
Orientation: L-T
Stress Ratio: 0.1

Yield Strength: 160 ksi


Ult. Strength: 170 ksi
Specimen Thk: 0.148 - 0.151 in.
Specimen Width: 3 in.
Ref: 86844

AK (MPaVin)
1

b I

10

40

' I Tl'l

100

' I'l'l'l

- Environment: H.H.A.; R.T.;


_
Frequency: 1. Hz

-H

___r

(2 of 4)

AK (MPaVin)

4)

10

40

100

' I 'I'l'l

Environment: H.H.A: R.T.:


Frequency: 20. Hz

1
~~

10

10

io"2

-3 EI

10

-=Jio >
10

10

10

40

100

AK (KsiVin)
da/dN (10-6in/cycle)

AK (KsiVin)

RMS %
Error
14.78

Life Prediction Ratio Summary


-r-

0.

.5

.8

1.25

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

0.0703
0.112
0.237
0.440
0.741
1.16
1.70

4.47 (min)
5.
6.
7.
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
45.10 (max)

0.603
0.653
1.08
1.64
4.11
7.84
15.1
29.4
52.4
89.5
149.
395.
1014.
1347.

7.86 (min)
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
50.
60.
63.06 (max)

10

AK (KsiVin)

2.

RMS %
Error
9.62

Figure 6.18.3.1.8
6-504

4.13
7.64
13.8
24.5
40.5
66.0
111.
209.

Life Prediction Ratio Summary


0.

.5

.8

1.25

Ti-6AI-6V-2Sn \
Condition/Ht: STOA
Form: 0.63 in. Plate
Specimen Type: CT
Orientation: LT
Stress Ratio: 0.1

Yield Strength: 160 ksi


Ult. Strength: 170 ksi
Specimen Thk: 0.148 - 0.151 in.
Specimen Width: 3 in.
Ref: 86844
(3 of 4)

AK (MPaVin)
1

- I

10

40

' I M'l'l

EF

(4 of 4)

AK (MPaVin)
4

100

' I MTI

10
i I ill

nrI

40
100
i 11 mi
10

Environment: 3.5ss NaCI; R.T.;


_
Frequency: 20. Hz

-Environment: 3.5* NaCI; R.T. -=j 10


_ Frequency: 1. Hz

10
.52

10"2

10" E

10

o
x>

10

10

10

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error
14.53

0.

.5

.8

100

1.25

0.151
0.223
0.499

4.61 (min)
5.
6.
7.
8.
9.
10.
13.
16.
20.
25.
30.
35.
39.72 (max)

Life Prediction Ratio Summary


i

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.552
0.660
0.999
1.49
2.19
6.04
13.9
33.8
80.2
164.
305.
528.
2094.
13672.

6.57 (min)
7.
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
50.
54.97 (max)

10

AK (KsiVin)

AK (KsiVin)

2.

RMS %
Error
12.57

1.48
2.19
3.05

6.46
11.1
19.5
34.0

53.7
78.2
105.

Life Prediction Ratio Summary

0.

.5

.8

1.25

Figure 6.18.3.1.8 (Concluded)


6-505

0.916

2.

^ Ti-6AI-6V-2Sn r
Condition/Ht: STOA
Form: 0.38 in. Plate
Specimen Type: CCP (max load specified)
Orientation: TL
Frequency: 10 Hz
Environment: H.H.A.; RT

- I

(1 of 2)
AK (MPaVin)
4
10
40
100
i I >|i|>|
| ' | M'l'l
-1
-=

10

-2

10
~~

fri o"
c

-3 |

10

zio

_4.T3

10
x>

_R h10

- I ' I Tl'l

XI

R
.-6

10
10
10

i , i,i,i,

10
4

10

40

10

JS

jff^

RMS %
Error
15.21

0.

.5

.8

10

\
10

X)
10

10

100

1.25

0.271
0.332
0.550

4.54 (min)
5.

6.
7.
8.

0.896
1.35
1.87
2.37
5.27
16.9
44.0
172.

9.
10.
13.
16.
20.
22.27 (max)

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.615
0.764
1.40
2.16
4.71
7.45
12.4
24.7
56.3
146.
421.
531.

Life Prediction Ratio Summary


i

10

_L

AK (KsiVin)

da/dN (10"6in/cycle)

7.71 (min)
8.
9.
10.
13.
16.
20.
25.
30.
35.
40.
41.04 (max)

i , i,u,

- i , i,i,i,

100

AK (KsiVin)
AK (KsiVin)

I ' I M'l'l

10

10

6^10-4

-z. 10
"a
tz

10

in i

10

X)

(2 of 2)

AK (MPaVin)
4
10
40
100
Stress Ratio: 0.5

Stress Ratio: 0.1

10

Yield Strength: 160.3 ksi


Ult. Strength: 167.8 ksi
Specimen Thk: 0.375 in.
Specimen Width: 5 in.
Ref: 90981

2.

RMS %
Error
16.67

Figure 6.18.3.1.9
6-506

Life Prediction Ratio Summary

0.

.5

.8

1.25

2.

I Ti-6AI-6V-2Sn h
Condition/Ht: STOA
Form: 0.13 in. Plate
Specimen Type: CCP (max load specified)
Orientation: TL
Stress Ratio: 0.1
Frequency: 10 Hz
(1 of 1)

AK (MPaVin)
4
10
i I i I i IT

Yield Strength: 137.4 ksi


Ult. Strength: 143 ksi
Specimen Thk: 0.125 in.
Specimen Width: 5 in.
Ref: 90981

AK (MPaVin)
1

40
100
i I i I MM

- Environment: H.H.A.; R.T.

10

40

100

b I ' I 'I'l'lI ' I 'I'll

10

1
-2

10

10

10

10

_0)

jD

io"2

o
_
6-10-4

-3 I

10

- 10"' E

10

10

x>
o

XI

-AT>

10

XI

o
x>

-6

10
-5

10

10

10
10

10
10
4

10

40

'

I I I III

100

da/dN (10"6in/cycle)

da/dN (10"6in/cycle)

AK (KsiVin)

3.15

5.98
10.8

16.7
23.2
29.9
42.3
46.9

Life Prediction Ratio Summary

RMS %
Error

Life Prediction Ratio Summary


i

0.

100

0.390
0.525
0.734
1.67

8.20 (min)
9.
10.
13.
16.
20.
25.
30.
35.
40.
50.
54.31 (max)

RMS %
Error
34.05

I I HU

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'

10

.5

.8

0.

1.25

Figure 6.18.3.1.10
6-507

.5

.8

1.25

2.

Ti-6AI-6V-2Sn fCondition/Ht: STOA


Form: 0.38 in. Plate
Specimen Type: CCP (max load specified)
Orientation: TL
Stress Ratio: 0.1
Frequency: 0.1 Hz
(1 of 1)

AK (MPaVm)
4

10

' I 'I'l'l

40

Yield Strength: 160.3 ksi


Ult. Strength: 167.8 ksi
Specimen Thk: 0.375 in.
Specimen Width: 5 in.
Ref: 90981

AK (MPaVin)
4

100

' I 'I'l'l

t I

10

40
100
1I I I Hill

' I 'I'l'l

10

-2

10

10
-3

10

o
\

o
o10"

-3 |

10

-5

10

_*/u

10

.-6

10

10

10
10
10
4

10

40

'

100

AK (KsiVin)

da/dN (10"6in/cycle)

Life Prediction Ratio Summary


a
-i

0.

I I I III

40

100

da/dN (10"6in/cycle)

1.37
1.73
2.38
5.97
13.7
26.4
57.8

8.30 (min)
9.
10.
13.
16.
20.
23.43 (max)

RMS %
Error
15.82

10

AK (KsiVin)

AK (KsiVm)
AK (KsiVin)

'

I I 11II

.5

.8

RMS %
Error

Life Prediction Ratio Summary


-r-

.5 .8

1.25

Figure 6.18.3.1.11
6-508

1.25

2.

This page intentionally left blank

6-509

EF

\ Ti-6AI-6V-2Sn r
Condition/Ht: STOA
Form: 0.38 in. Plate
Specimen Type: PTSF (max stress specified)
Orientation: L-S
Stress Ratio: 0.1

(1 of 3)

AK (MPaVin)
1

10

b I ' I 'I'l'l

Ti

Yield Strength: 130 ksi


Ult. Strength: 167.2 ksi
Specimen Thk: 0.372 - 0.374 in.
Specimen Width: 5 in.
Ref: 90981

40
100
i i Mm

10

- I 'I 'I'l'l

-Environment: H.HA; R.T.;


_
Frequency: 0.1 Hz

-=|

10

-2
10

10
10
2

io"
o
\
-3 |
10

(2 of 3)

AK (MPaVin)
40

100

I ' I 'I'l'l

_i

Environment: H.H.A.; R.T.;


_ Frequency: 10. Hz

z. 10

-r

2 <o

10"

o
u 10
\
c

10

Z 10
\
o
"

-=

10

10
10

40

~ I ,

I.I.I,
4

100

da/dN (I0'6in/cycle)

RMS S
Error
9.58

5.64
8.89
22.6
65.9
110.

Life Prediction Ratio Summary


0.

.5

.8

100

0.592
2.53

9.04 (min)
10.
13.
16.
20.
25.
30.
35.
39.96 (max)

1.94
4.44

40

da/dN (10"6in/cycle)

AK (KsiVin)

0.708
0.949

8.70 (min)
9.
10.
13.
16.
20.
25.
30.
34.23 (max)

I , I,LI,

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

m^
u

10

10

'

10

10

=1
Xi

iI
*

-6

10

10"

-z.

x>

"

X>

JB

1.25

RMS %
Error
12.37

Figure 6.18.3.1.12
6-510

7.01
5.18
7.63
22.0

51.7
96.5
140.

Life Prediction Ratio Summary


-T"

0.

.5

.8

1.25

-\ Ti-6AI-6V-2Sn
Condition/Ht: STOA
Form: 0.38 in. Plate
Specimen Type: PTSF (max stress specified)
Orientation: LS
Stress Ratio: 0.1

- I

10

40
100
TI I I I IMI

' I M'l'l

Yield Strength: 130 ksi


Ult. Strength: 167.2 ksi
Specimen Thk: 0.372 - 0.374 in.
Specimen Width: 5 in.
Ref: 90981

(3 of 3)

AK (MPaVin)

EF

AK (MPaVin)
1

t I

10

' I M'l'l

40

100

' I M'l'l

-Environment: 3.5ss NaCI; R.T.; -=\ 10


Frequency: 10. Hz

10

10
10

10

io"2

6-10-4
10

"D

10

-J10 >

TJ

10
10
10
10

10
4

10

40

LA
4

100

da/dN (I0~6in/cycle)

Life Prediction Ratio Summary


i

0.

40

100

da/dN (10*6in/cycle)

AK (KsiVin)

2.38
2.38
2.92
10.0
22.6
31.7
48.6
69.8
50.0

8.98 (min)
9.
10.
13.
16.
20.
25.
30.
32.63 (max)

RMS %
Error
5.87

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I I I I III

I I I I III

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


i

0.

2.

Figure 6.18.3.1.12 (Concluded)


6-511

.5

.8

1.25

i Ti-6AI-6V-2Sn r
Condition/Ht: STOA
Form: 0.38 in. Plate
Specimen Type: PTSF (max stress specified)
Orientation: TS
Frequency: 0.1 Hz
Environment: H.H.A.; RT
(1 of 2)

AK (MPaVin)
4

10

40

- I ' I 'I'l'l

I ' I Tl'l

_L

10

40

' I 'I'l'l

100

' I 'I'l'l
10

Stress Ratio: 0.5

(2 of 2)

AK (MPaVin)

100

Stress Ratio: 0.1

10

Yield Strength: 130 ksi


Ult. Strength: 167.2 ksi
Specimen Thk: 0.373 - 0.374 in.
Specimen Width: 5 in.
Ref: 90981

10
10

10
-3

10

-S2
2
10"

T>
XI

10

10

IP

t1

^io-<

10

10

10
10

10
10

"I.I ,l,l.
4

1 , 1,1,1,

10

40

I I.I.I.I

10

100

da/dN (10"6in/cycle)

RMS %
Error
14.14

0.

.5

.8

40

100

2.79
2.47
1.83
16.6
36.5
48.8
102.

8.90 (min)
9.
10.
13.
16.
20.
22.70 (max)

Life Prediction Ratio Summary


I

. I.I,I.

da/dN (10"6in/cycle)

AK (KsiVin)

0.608
0.630
0.875
4.81
19.4
39.8
70.4
148.
131.

8.60 (min)
9.
10.
13.
16.
20.
25.
30.
33.13 (max)

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

10

10

10

-*"

-3 I

10

_iX)
10
o

10

io"2

-3 |
10 E

Sa
cT

b^io-+
c

10

1.25

2.

RMS %
Error
26.12

Figure 6.18.3.1.13
6-512

Life Prediction Ratio Summary


0.

.5

.8

1.25

I-'

2.

\ Ti-6AI-6V-2Sn r
Condition/Ht: STOA
Form: 0.38 in. Plate
Specimen Type: PTSF (max stress specified)
Orientation: T-S
Frequency: 1 Hz
Environment: 3.5$ NACL; RT

- I

10

40

' I U'PIf

Yield Strength: 156.5 ksi


Ult. Strength: 167.8 ksi
Specimen Thk: 0.375 in.
Specimen Width: 5 in.
Ref: 90981

(1 of 1)

AK (MPaVin)

AK (MPaVin)
1

100
TTTm

= I

10

' I 'I'l'l

40

100

' I 'I'l'l

=
10

Stress Ratio: 0.1

10

10

10
10

10
_QJ

o
o 10

o
6^10~

10"

a;

C>

10~

"I

^S

-5

10

10

m~ ^
u
T3

10

10

10
10

10

10
10

10

10

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

1.28
1.30
5.25
28.1
100.
168.
275.
470.

9.26 (min)
10.
13.
16.
20.
25.
30.
35.
40.
45.85 (max)

RMS %
Error
22.11

10

AK (KsiVin)

AK (KsiVin)

674.
2109.

Life Prediction Ratio Summary


i

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


i

i-'

2.

0.

Figure 6.18.3.1.14
6-513

.5

r-

.8

i--

1.25

2.

\ TI-6AI-6V-2Sn r
Condition/Ht: 1300F 2HR
Form: 2 in. Forging
Specimen Type: TDCB
Orientation: LT
Yield Strength: 146 ksi
Ult. Strength:

Specimen Thk: 1.25 in.


Specimen Width: 5.5 in.
Ao:
Klscc: 31 - 32 ksi
Ref: 84360

Kmax (MPaVin)
4

- I

10

' I 'I'l'l

40

of 2)

100

' I M'l'l

Environment: 3.5* NaCI;


_ R.T.

' I M'l'l

40

100

' I M'l'l

Environment: JP-4 Jet Fuel;


_ R.T.

"d10

10

10

10

10
[

5?

-r:

10 2

Ci

k-

-=

VI

.'I
*. 10

-J10
>
-=

10
10
-1

10

-= 10

-3

10

II I I

10

T7

XI

10

10

110

T3

10

10

+^10

= I

10
~

10

(2 of 2)

Kmax (MPaVin)
1

10

-= 10

I J.I.I,

10
4

10

0
40

10

100

33.10 (min)
35.
40.
42.70 (max)

RMS %
Error
>100.0

da/dt (10"3in/hour)

Kmax (KsiVin)
33.70 (min)
35.
40.
41.50 (max)

0.210
3.68
5322.

3848.

RMS %
Error
>100.0

Figure 6.18.3.2
6-514

ipl i 1111

40 1 00
Kmax: (Ksivin)

Kmax (Ksivin )
Kmax (KsiVin)

I I.I.I
1o

da/dt (10"3in/hour)
1.79
6.54
1553.
631.

Ti-6AJ-6V-2.5Sn

mMm

swssoss;

ill

s
p

:*:-:--:-:::::;:*:::::

I;!;!;!;!;!;!;!:!;!;!;!;!:!::

s
e

:: e>
... '.:o

CO
CO

CO

mm

CO

wmm

rH

-f

::::::::::::::::!:'::::::::::

8
M

S'S
s

S8SBKS88S

-* ~

CO

2 B

05

0)

to

P4

llllll

CO
05
rH

rH

in
io

J-iSSSS::;:::;::::::

lilll

'
CM
<N

io

.6 "
<M

T-H

ta

IO

wmm
.rH

rH

H3
0

>

J5

a 3.S
0
~
0
0.

CO

10

lllil

la
figa

t-

&::i:::::::::*::::::::
rH

4
CO

CO

5
us

rH
CO
OS
O

111

^^

~*

rH

i3

t-

mm

Test
Time
(min)

HP

CO

&

p*

00

Q
fc

>

V.

' J

u> :

W.-W*:*v.:

**W*W:**

HPI

|l

<i

iiiiii
#o
o
w-

CQ

Q
H

0
h
eg

OS

|||||

iili

1"S
OH

1-H

-3 fa

0
0

? 5
#-Si
? e
CO ?*

w J5

B.

tJ . o
0 -S

pe
K

s a&
*o Sa

CO
rH

iH

CN

CO

to

co

Ol

lO
1-H

09
0

Hi
03

rH

p<

EH

EH

CO

-B
Cl

EH

H
OS

E-;

EH

OH

OH

OH

fa

fa

fa

as

wH

B
M
OS

OH

fc fa

fits

C
0
o

<

B5

8.
to
C

ja

"S

Its
0 V

q
<
CO

fa

fa

TH

CO
rH

o
o

cyo

<
j-,

>-

rH ^
fe fa

SS
rH

a
OS

M
OS
n

OB

6-515

Ti-6A12Sn4Zr6Mo \

I
is
rfi

Si
tf
z
o

EO

H
Q

8-
Sen

E8

CO

'i>

o
E-

E-

B6E
ggt

OS

PS

DS

E-

es

<E*

rf

S3 E

f- s

ft.

o
a

in

a
<
CO
,< s S e os

is-s8
SQ|2

.i H S
SB
fc en
pa Z

SE

03

H OS E O
03 0, 5 - .
O <S J Cx fc

So
5*
E2
oa s

55
SP

3 fc-

6-516

gsg<oses

H 05 C ^ K SI
oa e- 5 Q - co

S
o
u

<s
#ri
EO 13
5 fe
B fe
8
o
z

Ti-6A12Sn4Zr6Mo

is
M

^i

rfi

ii
i

OS
0)

a ea

ii*

O
CO

9s?

P. o

E"

eg*

as

EOS

E-

si

53 B
SO
g

o
B
Ho.,
m 2

&Q2
3

ID

o<

&
H ro J

pa S
8
fe

<
2
H < o
O

5SS

2 I

u 6

2,1
m *" S

9] n n

3E
32o

<

b y as
w !j

Sg

U3 < K
M

2 <o
2 K &

< ~ J
m EH

D
ca

E* & EU

sas
ooo

U O O
TO

g"8

fc s o

355

Sap
33s
Q
a
B
a

o
2

6-517

Ti-8i&lMolV

o
o
:5s:

*-<

to

t-

CO
CO

co

CO

CO

a
&

::>:::::**:::-::::::-:::

*>

CO

CO

IN

CO

CO

11

U3

CO
CO

CO

CO

IIII1

JO

(Hz)

si

cM

co

cc

CO

CD

CONDITION/
HEAT TREATMENT

ffl

PRODUCT

^ft &;;:;.;.

CO

O
CO

o
CO

CO
CO

3
CO

CO

o
d

Q
K

5
w
0-

co
2
X

E-

K
H
X
CO

Eca
63

X
to

E-i
U
M
X
to

3
Q
Cd

o
US

<

<
s

u
&a

a.
CO

2
3
N
CO

6-518

Ti-8Al-lMo-lV

ssos
K

O
H

o
SSQK
/

fa

T>

II

3
OS

I
03

fa p4
PS p

c4
1-H

N
CO

fa

02
fa !
O fa
02

SUI

H
Z
fa

itpll

SSSS^jS

:SSB5BSS*S

III
iiin
iJlli;

HI
liltll

z
o
tf

fa

O1^

is

o
P3

fa
hJ

o
o
fa
P

A* '

Z
fa
fa
Q>

S 4

O
2

l? "

ilti
og
:::

::

g
o
b.

: : : : : : : : : ::

: : :flg: : J!W: : : : : : : : : : :

ti

z
o
t-4
H

<

z
fa
NH

H
Z

ipfaiill WM

S
op ill
f< >

si
ZH
Ofa
Q5

HI

<
X

fc.
o

l
as

in a
fc.

CO
OS

ffl

6-519

Ti-8Al-lMo.lV

ns

12

<
a

is
M

t^e

rfl

eg-,
z
2So
H

Q
i-i

CO

Ed

a.00

B~
!i*

pg
a, o

ii

o
o

Si

6-520

Ti-8Al-lMo-lV

is

rfi
5>

is
M

J*

Ss
N

Si'
00

Hi
|i

u
w
eu
00

l-S*

9es
H g

a. o

6-

as

si

D
Q

a.

SB

6-521

Ti-8Al-lMo.lV
as

2>

rf

*;

5>

j*

rf
O

00

s
5
o
W

li

1*

d
s

Id

I
2*

9pi

H
&

J
fi

ggafc
7

8a.

3'

6-522

This page intentionally left blank

6-523

\ Ti-8AI-1Mo-1V I
Condition/Ht:
Form: 0.05 in. Sheet
Specimen Type: CCP (max stress specified)
Orientation: L-T
Frequency: 0.1 12 Hz
Environment: LAB AIR; RT
(1 of 1)

AK (MPaVin)
4

10

Yield Strength: 119.5 ksi


Ult. Strength: 134 ksi
Specimen Thk: 0.05 in.
Specimen Width: 6 in.
Ref: MA011

AK (MPaVin)
1

40
100
ni I i I i|i|

i 'i'i'i

- I

10

' I 'I'I'I

40

100

' I 'I'I'I

10

Stress Ratio: 0.02

-2

10
-i

10

10
10
2

io"

10~

-S2
o

o
\

6^10-

-3 I

10

10~

'1

^-^

10
10

<o

iff ^
o
"o

_K
10
10

10
-7

10

10

10
10
4

10

40

100

AK (KsiVin)
da/dN (10-6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary

100

da/dN (10"6in/cycle)

AK (KsiVin)

.5

RMS %
Error

Life Prediction Ratio Summary

i-'

r-

0.

40

0.621
0.824
1.22
1.70
2.28
7.75
13.5
37.3
78.7
243.
589.
1243.
2281.

6.38 (min)
7.
8.
9.
10.
16.
20.
30.
40.
60.
80.
100.
118.36 (max)

RMS %
Error
34.74

10

AK (KsiVin)

.8

1.25

0.

2.

Figure 6.21.3.1.1
6-524

.5

.8

1.25

This page intentionally left blank

6-525

^ Ti-8AI-1Mo-1V
Condition/Ht: 1825F 1HR AC 1350F 2HRS AC
Form:
Specimen Type: KB Bar
Orientation: L-T
Frequency: 0.3 Hz
Environment: LA AIR; RT
(1 of 3)

AK (MPaVin)
4

l- I

10

Yield Strength: 120 ksi


Ult. Strength:
Specimen Thk: 0.251 - 0.253 in.
Specimen Width: 0.75 in.
Ref: GE006

40
100
TI I I MIH

' I 'I'l'l

(2 of 3)

AK (MPaVin)
10

40
100
i I i MM

10

Stress Ratio: 0.
10

10
-3

10

-2-n

jo
o
6^10-+

-31

10

10
10

T3

10
10

10
10
' i i i i n

10

I I.I.I.

10

40

100

AK (KsiVin)

16.
20.
25.
30.
31.31 (max)

RMS %
Error
14.89

Life Prediction Ratio Summary


i

.5

.8

100

1.25

0.0326
0.0996
0.229
0.341
0.508
1.86
4.10
25.1

6.37 (min)
7.
8.
9.
10.
13.
16.
19.64 (max)

2.15
4.13
10.2
23.8
74.2
114.

13.50 (min)

40

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (10_6in/cycle)

AK (KsiVin)

10

AK (KsiVin)

RMS %
Error
18.30

Figure 6.21.3.1.2
6-526

Life Prediction Ratio Summary


I

.5

.8

1.25

i--

2.

^ Ti-8AI-1Mo-1V h
Condition/Ht: 1825F 1HR AC 1350F 2HRS AC
Form:
Specimen Type: KB Bar
Orientation: LT
Frequency: 0.3 Hz
Environment: LAB AIR; RT

- I

10

I I llllll

40

Yield Strength: 120 ksi


Ult. Strength:
Specimen Thk: 0.251 - 0.253 in.
Specimen Width: 0.75 in.
Ref: GE006

(3 of 3)

AK (MPaVin)

AK (MPaVin)
4

100

' I 'I'l'l

-i

- I

10

40

I I 'I'l'l

100

' I 'I'l'l

10

10

10

10

10

10
v
o

-1
10

10

- Stress Ratio: 0.54

^10"4
\
c
_

10

o
^10"4
\
c
_

\
-=: 10

zio
o

_K I

10
-= 10

10 \
o

XI

10

10

10

10

-7

10

10

10

10
10

T>

~ I , I,I,I,
4

I , 1.1,1,

10

40

10

da/dN (10'6in/cycle)

100

da/dN (10"6in/cycle)

AK (KsiVin)

Life Prediction Ratio Summary


0.

40

2.48
6.62
19.0
21.9

10.39 (min)
13.
16.
16.74 (max)

RMS %
Error
8.96

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

1 , LLL

" i i iii.ii

100

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


i

!-

0.

2.

Figure 6.21.3.1.2 (Concluded)


6-527

.5

.8

1.25

2.

H Ti-8AI-1Mo-1V h
Condition/Ht: 1830F 1HR WQ 11 OOF 8HRS AC
Form: 1 in. Forging
Specimen Type: CCP (max load specified)
Orientation: C-R
Frequency: 30 Hz
Environment: LAB AIR; RT
(1 of 1)

AK (MPaVin)
4
1

10

40
100
1 1 ' M Ml

I MM1

Yield Strength: 135.5 - 145.8 ksi


Ult. Strength: 148.5 - 159.3 ksi
Specimen Thk: 0.078 - 0.08 in.
Specimen Width: 1.75 in.
Ref: PW002
AK (MPaVin)
4
10
I I ' I'I'l

40

100

' I 'I'M
10

Stress Ratio: 0.1


10

10
10

u
o^10-4
10

10

-=ho >
x>
10
10
-7

10

10
10
4

10

40

100

AK (KsiVin)

AK (KsiVin)
da/dN (10-6in/cycle)

AK (KsiVin)
5.
6.
7.
8.

da/dN (10-6in/cycle)

0.824
1.14
3.04

9.
10.
13.
16.
19.11 (max)

6.83
9.55

Life Prediction Ratio Summary


0.

AK (KsiVin)

0.0347
0.130
0.277
0.433
0.604

4.09 (min)

RMS %
Error
31.78

I Mill
40
100

I [Mill
4
10

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


0.

2.

Figure 6.21.3.1.3
6-528

J3

1.25

This page intentionally left blank

6-529

-J 1 i 8AI-1MO-1V

Condition/Ht: DA
Form: 0.05 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: LT
Frequency: 1 30 Hz
Environment: LAB AIR; RT

AK (MPaVin)
4

10

40

- I ' I M'l'l

of 4>

I ' I 'l'l'l

"~~

10

o
\

-3|
10 E

"O

io"3
a>

^
=

^S

2 10"5

Z10"5

\
o

10

>

10

10

10
40
AK (KsiVin)

RMS %
Error

10""

100

.5

r '

.8

1.25

I , I,I,I,

" I , I,I,I,
1

Life Prediction Ratio Summary


0.

10

10

da/dN (10"6in/cycle)

AK (KsiVin)

~o

-6

-6

>

io"7

10

I , l,l,l,

^~'

-5

~~zz

"1,1 ,1,1,

10

-6

-5

m-8

o
\

10

io"7

io"2
10

T3

-6

10

n/cyc

10

-1

**s

' I ' ITI

^_^

100

10"2
-1

40

Stress Ratio: 0.25

10

o
fri o"4
\
c

10

- I ' I ' I'l'l

io-3

1
1

(2 of 4)

AK (MPaVin)

100

Stress Ratio: 0.
la"2

Yield Strength: 136.3 ks i


Ult. Strength: 150.7 ksi
Specimen Thk: 0.05 in.
Specimen Width: 2 in.
Ref: 86099

10
40
AK (KsiVin)

6
da/dN (10 " in/cycle)

AK (KsiVin)

RMS %
Error

100

Life Prediction Ratio Summary

>

0.

2.

Figure 6.21.3.1.4
6-530

.5

.8

1.25

2.

\ Ti-8AI-1Mo-1V
Condition/Ht: DA
Form: 0.05 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: L-T
Frequency: 1 30 Hz
Environment: LAB AIR; RT

4
1

10

40

I M'l'l

Yield Strength: 136.3 ksi


Ult. Strength: 150.7 ksi
Specimen Thk: 0.05 in.
Specimen Width: 2 in.
Ref: 86099

(3 of 4)

AK (MPaVin)

Stress Ratio: 0.43

(4 of 4)

AK (MPaVin)

100

' I Tl'l

I
10

10

' I M'l'l

40

100

' I M'l'l

Stress Ratio: 0.67

-2

10

10

10
-3

10

10

Q)

\
10

_c

Z 10
a

-s-

10

10~

o
_
0-10-4

-3 |

TJ

=!

10

10

o
10

-=]io >

>,
o

1-

10"

tz

10-*^p
\

-5

v x

-z.

10

10

10

10

10

10

10
i I i I in

'

10

10

I I I III

40

100

Life Prediction Ratio Summary


0.

.5

.8

10

40

100

AK (KsiVin)

da/dN (10-6in/cycle)

AK (KsiVin)

I l I III!

i i i nil

AK (KsiVin)

RMS s
Error

u
x>

10

10

da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error

Life Prediction Ratio Summary


.5

1.25

Figure 6.21.3.1.4 (Concluded)


6-531

.8

1.25

1 Ti-8AI-1Mo-1V I
Condition/Ht: DA
Form: 0.05 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: LT
Frequency: 43 Hz
Environment: LAB AIR; RT
(1 of 1)

AK (MPaVin)
1

10

Yield Strength: 140 ksi


Ult. Strength: 149.2 ksi
Specimen Thk: 0.064 in.
Specimen Width: 3 in.
Ref: 86099

40

AK (MPaVin)
4

100

10

40

b I ' I 'IT

b I ' I 'I'l'lI ' I 'I'l'l

100

' I 'I'l'l
10

-2

10

10

10

u
6-10-4
10

-5

10

L."0

10

-0
10

10
10
10
.-8

10
4

10

40

I.I.I.
4

100

da/dN (10"6in/cycle)

Life Prediction Ratio Summary


CD
1

0.

100

da/dN (10-6in/cycle)

AK (KsiVin)

5.41
7.92
10.5
13.6
25.8
61.9
239.
792.
1190.

17.97 (min)
20.
25.
30.
35.
40.
50.
60.
62.14 (max)

RMS %
Error
13.38

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I . Ml

10

.5 .8

RMS %
Error

1.25

Life Prediction Ratio Summary


0.

2.

Figure 6.21.3.1.5
6-532

.5

.8

-1

1.25

This page intentionally left blank

6-533

\ Ti-8AI-1Mo-1V I
Condition/Ht: DA
Form: 0.05 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: L-T
Frequency: 1 30 Hz
Environment: LAB AIR; RT
(1 of 4)

AK (MPaVin)
1

- |

10

40

' I M'l'l

Yield Strength: 136.3 ksi


Ult. Strength: 150.7 ksi
Specimen Thk: 0.05 in.
Specimen Width: 4 in.
Ref: 86099

100

' I M'l'l

Stress Ratio: 0.

(2 of 4)

AK (MPaVin)
4

- I
10

10

40

' I M'l'l

100

' I M'l'l

Stress Ratio: 0.25

10

10

10
-1

10

10

-3

10

10

fri0"+

10-*

10
-

cP

-5

10

_*.-o
10

xi

X>

10

eP

z
Jio >
x>

XI

_K

10

10

-5

~410

10

10

10

-6

10

10
'

10
4

10

10

l i l ili

40

Li

i i im

100

RMS %
Error

0.

.5

.8

100

da/dN (1Q-6in/cycle)

AK (KsiVin)

da/dN (l0-6in/cycle)

Life Prediction Ratio Summary


i

1 I III!

40

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'

10

RMS %
Error

1.25

Figure 6.21.3.1.6
6-534

Life Prediction Ratio Summary


I

0.

.5

.8

1.25

1~

2.

Ti-8AI-1Mo-1V h
Condition/Ht: DA
Form: 0.05 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: LT
Frequency: "1 30 Hz
Environment: LAB AIR; RT

10

40

(4 of 4)

AK (MPaVin)
1

100

_ I 11 >lllll
I I I 'nil
- Stress Ratio: 0.43

-1

10

40
100
-rrrn-

b i ' Mi'i'iT

TT

Stress Ratio: 0.67

10

10

-3

10

10

~~

JE
o
o 10
\
c

Z. 10
"O

tZ

a;

io" ^

10
o
o 10

o
\

'1

10~

'

10

m~^
u

^10
>

_B :

;/

XI

10

10

10

10
-7

10

10

10

"O

Yield Strength: 136.3 ksi


Ult. Strength: 150.7 ksi
Specimen Thk: 0.05 in.
Specimen Width: 4 in.
Ref: 86099

(3 of 4)

AK (MPaVin)

:
10

10

10

10
-

10

i ,I,I,I,
4

I , I,I,I,

10

40

10

100

RMS %
Error

da/dN (10"6in/cycle)

Life Prediction Ratio Summary


i

0.

.5

.8

10

1111 ii

40

100

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i I i 11 h

1.25

RMS %
Error

Life Prediction Ratio Summary


i

0.

.5

.8

1.25

Figure 6.21.3.1.6 (Concluded)


6-535

da/dN (10"6in/cycle)

AK (KsiVin)

2.

\ Ti-8AI-1Mo-1V I
Condition/Ht: DA
Form: 0.05 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: LT
Frequency: 1 30 Hz
Environment: LAB AIR; RT
(1 of 4)

AK (MPaVin)
1

Yield Strength: 136.3 ksi


Ult. Strength: 150.7 ksi
Specimen Thk: 0.05 in.
Specimen Width: 7.992 in.
Ref: 86099
(2 of 4)

AK (MPaVin)
1

10

40
100
11 I 1 111 I
=q
I ' I M'l'l

10
Stress Ratio: 0.

- I

10

' I M'l'l

40

100

' I M'l'l

10

Stress Ratio: 0.25


10

10

-1

10

10
-3

10
O

6^1 o"+

.s?

10

10
o
6-10-4

-5

z:

-5

10

10

-3 I

10

10
-

_.iX>

10

-6

10

10

10

10
10

10

10

10
11 III

10
4

10

10

1 11 in

40

RMS %
Error

da/dN (10-6in/cycle)

Life Prediction Ratio Summary


1

.5

.8

40

100

RMS %
Error

Life Prediction Ratio Summary


0.

2.

Figure 6.21.3.1.7
6-536

da/dN (10"6in/cycle)

AK (KsiVin)

1.25

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

I I I I III

I I I I II!

100

.5

.8

1.25

H Ti-8AI-1Mo-1V
Condition/Ht: DA
Form: 0.05 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: L-T
Frequency: 1 30 Hz
Environment: LAB AIR; RT

10

40

Yield Strength: 136.3 ksi


Ult. Strength: 150.7 ksi
Specimen Thk: 0.05 in.
Specimen Width: 7.992 in.
Ref: 86099

(3 of 4)

AK (MPaVin)

100

i ' i M'l'ir

(4 of 4)

AK (MPaVin)

-II I 11 nil

- I
10

Stress Ratio: 0.43

10

40

' I 'I'l'lI

100

' I'I'l'l

10

Stress Ratio: 0.67


10

10

10

10
-3

10

10
u
o 10

VI

10

jo

b^io-4

10

"o

10

10

io"2

10

.."O

10

_fi
10
10
10

10

10

10

LL

i 11

i I iI Mi

10

40

Li

,1,1,

10
4

100

da/dN (10"6in/cycle)

AK (KsiVin)

I , 1,1,1

10

40

100

AK (KsiVin)

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

2.38
2.54
5.76
11.3
20.3

9.65 (min)
10.
13.
16.
18.26 (max)

RMS %
Error

-5

10

10

Life Prediction Ratio Summary


.5

.8

1.25

RMS %
Error
2.13

Life Prediction Ratio Summary

0.

Figure 6.21.3.1.7 (Concluded)


6-537

.5

.8

1.25

2.

^ Ti-8Ai-iMo-iv h
Condition/Ht: DA
Form: 0.05 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: LT
Frequency: 20 - 30 Hz
Environment: LA AIR; RT
(1 of 4)

AK (MPaVin)
1

10

40

' I M'l'l

Yield Strength: 133.7 ksi


Ult. Strength: 152.1 ksi
Specimen Thk: 0.05 in.
Specimen Width: 7.992 in.
Ref: 86099

100

' I Tl'l

Stress Ratio: 0.

(2 of 4)

AK (MPaVin)
4

b I
10

10

40

' I 'I'l'lI

100

' I 'I'l'l

Stress Ratio: 0.25

-2

10

10

10

10

10
-3

10

10

10"
o 10

"ET

-3 I

10

o
G^10-4

-3 I

-5

-I

-4^
10

"o

^110 >

>

_s

JEfi

10

10

10

cP

10

10

10

10
-7

10

10

10

10

10

'

'

i 1 1 in

10

10

1 1 1 in

40

100

i i i mi
4
10

RMS %
Error

da/dN (10"6in/cycle)

Life Prediction Ratio Summary


-1

0.

.5

.8

AK (KsiVin)

RMS %
Error

1.25

40

100

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

'

da/dN (10-6in/cycle)

Life Prediction Ratio Summary


i-'

.5 .8

2.

Figure 6.21.3.1.8
6-538

1.25

2.

] Ti-8AI-1Mo-1V h
Condition/Ht: DA
Form: 0.05 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: LT
Frequency: 20 - 30 Hz
Environment: LAB AIR; RT

10

i- i ' i M'l'i

40
-|

Yield Strength: 133.7 ksi


Ult. Strength: 152.1 ksi
Specimen Thk: 0.05 in.
Specimen Width: 7.992 in.
Ref: 86099

(3 of 4)

AK (MPaVin)

(4 of 4)

AK (MPaVin)
4

100

10

40

-PTTT

I I I MM

10

Stress Ratio: 0.43

100

' I 'I'l'l

Stress Ratio: 0.67

10

10
10

10

-no"2

.2?

o
^10"+

o 10

10

10

Z 10

T3

10

Jio >

10

10

10

10

10

10

10

10
-8

10

I llll

10

1A

'

40

100

10

AK (KsiVin)

da/dN (10"6in/cycle)

40

100

da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error

Life Prediction Ratio Summary


i

.5 .8

10

AK (KsiVin)

Life Prediction Ratio Summary

0.

I I i I ill

I I I hi

AK (KsiVin)

RMS %
Error

10

10

10

"O

0.

1.25

Figure 6.21.3.1.8 (Concluded)


6-539

.5

.8

1.25

2.

\ Ti-8AI-1Mo-1V r
Condition/Ht: DA
Form: 0.05 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: L-T
Frequency: 1 - 30 Hz
Environment: LAB AIR; RT
(1 of 4)

AK (MPaVin)
4

- I

10

40

' I M'l'l

Yield Strength: 136.3 ksi


Ult. Strength: 150.7 ksi
Specimen Thk: 0.05 in.
Specimen Width: 20 in.
Ref: 86099

100

' I M'l'l

Stress Ratio: 0

(2 of 4)

AK (MPaVin)
4

- I

10

40

i I M'l'l

100

' I M'l'l

Stress Ratio: 0.25

10

-= 10

-2

10

10

10

10

-3

10

10
jU

0
a

10~ y

O-10\

SMO-

J10

z 10

10

TJ

\
o
" -sl-

/
L_

'1

'

z
CZ

10 \
u
-0

10

~*

10
-7

10
'

1 t i in

40

10

I , M,l,

10

10

10

III I

10

10

100

40

33.3
35.0
51.1
72.1
161.
435.

29.33 (min)
30.
35.
40.
50.
59.13 (max)

Life Prediction Ratio Summary


0.

.5

.8

1.25

100

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (10'6in/cycle)

AK (KsiVin)

10

AK (KsiVin)

AK (KsiVin)

RMS %
Error

10"

T3

10

10

2
10"

*~~

RMS %
Error
2.98

Figure 6.21.3.1.9
6-540

Life Prediction Ratio Summary

0.

.5

1-1

.8

1.25

2.

^ Ti-8AI-1Mo-1V r
Condition/Ht: DA
Form: 0.05 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: LT
Frequency: 1 30 Hz
Environment: LAB AIR; RT

10

- I I I 'nil

40

Yield Strength: 136.3 ksi


Ult. Strength: 150.7 ksi
Specimen Thk: 0.05 in.
Specimen Width: 20 in.
Ref: 86099

(3 of 4)

AK (MPaVin)
Stress Ratio: 0.43

100
10

10

10

10

10
_

io"2

10

T3

Z 10
a
tr

o
o 10

o
\

-3 |

10

Z 10

"o

40

Stress Ratio: 0.67

-2

o^10-+

10

-1

10

JP
o

(4 of 4)

AK (MPaVin)

100

I ' I 'ITI

10 \
o

.olIO

"o

:
.olIO

10

Jio
>

10

:
10

10

10

10
10

i 1 11 ill
4
10

i , ij.i,
40

10

100

10

40

100

AK (KsiVin)

da/dN (10"6in/cycle)

AK (KsiVin)

i , i,i,i,

- i , i,i,i,

AK (KsiVin)

RMS %
Error

Life Prediction Ratio Summary

da/dN (10"6in/cycle)

AK (KsiVin)

RMS %
Error

Life Prediction Ratio Summary

!-

.5

.8

1.25

0.

2.

Figure 6.21.3.1.9 (Concluded)


6-541

.5

.8

1.25

I Ti-8AI-1Mo-1V h
Condition/Ht: MA
Form: 0.02 in. Sheet
Specimen Type: CCP (max load specified)
Orientation: L-T
Frequency: 43 Hz
Environment: LAB AIR; RT
(1 Of 1)

AK (MPaVin)
4

10

Yield Strength: 154.9 ksi


Ult. Strength: 159.2 ksi
Specimen Thk: 0.018 in.
Specimen Width: 3 in.
Ref: 86099

AK (MPaVin)
1

40
100
TI I > I'M

-IM 'I'l'l

10

b I ' I 'I'l'l

40

100

I ' I 'I'l'l

10

Stress Ratio: 0.1

-2

-2

10

10

10

10
-3

10

10
v
o

-m

6-10-

io"2

_
4

10
x
\
o
~

J2

_a)
o

io10

10

10

xi

-e r10

_
10

10

10

o
x

-5

_fi
10

10

10
10

10

10

10
.-8

10

I Mllll
40
100

' i i i HI
4
10

10

'

0.

100

6.85
7.30
10.7
23.0
56.6
71.1

Life Prediction Ratio Summary

o
i

40

da/dN (10"6in/cycle)

AK (KsiVin)

da/dN (10_6in/cycle)

19.10 (min)
20.
25.
30.
35.
39.05 (max)

RMS %
Error
29.51

10

AK (KsiVin)

AK (KsiVin)
AK (KsiVin)

i I Hi

i i 11 n

.5

.8

1.25

RMS %
Error

Life Prediction Ratio Summary


0.

2.

Figure 6.21.3.1.10
6-542

.5

.8

1.25

This page intentionally left blank

6-543

i1 T i 8AI-1MO-1V I
Condition/Ht:
Form:
Specimen Type: SENT
Orientation:
Yield Strength:
Ult. Strength:

Specimen Thk:
Specimen Width:
Ao:
K]scc:
Ref: 82651

max (MPaVin)
1

10

40

~ 10

- I

10

' I ' ITI

40

100

' I 'ITI

101

102

m\

|io

10
-

pf

10

10

i-

3
E

10

i_

\
i E

10
\
c

uJ^
iir

_1

-M

-M10
TO

L_

I
^-^

-^10
a

\
o

\
-2
102

10
-1

-1

10

10

10"3

ID'3

-2

10

IQ"2
in"4

101

\
c

10

- Environment: Dry CH2CI2

10

"

(2 of 5)

Kmax (MPaVin)

100

Environment: Dry CCI4

102

5)

~ I , 1,1,1,
1

10

i , LI,I,
40

m"4 -

100

28.00 (min)
30.
35.
40.
50.
60.
70.
74.50 (max)

1 , 1,1,1,

40

10

100

Kmax (Ksivin)

Kmax (KsiVin)
Kmax (KsiVin)

I , I,I,I,

da/dt (10"3in/hour)

Kmax (KsiVin)

581.
751.
1259.
1854.
3149.
4395.
5470.
5887.

RMS %
Error

RMS %
Error
19.99

Figure 6.21.3.2.1
6-544

3
da/dt (10" in/hour)

Ti-8AI-1Mo-1V r
Condition/Ht:
Form:
Specimen Type: SENT
Orientation:
Yield Strength:
Ult. Strength:

Specimen Thk:
Specimen Width:
Ao:
Kjscc:
Ref: 82651
(3 of 5)

Kmax (MPaVin)
4

- I

10

' I 'I'l'l

40

100

' I I * IM

10

10

10

10

<P^]

110

10

,0

lo't

-M10

40

100

1 ' 1 'I'l'l

10 \
o
T3

10

J 10 0

X)

/
&

\
_c

\
o

_,
-2

-1
10

-3

-2

10
=

10

10

10
-2

10

10

~ I , I,I,I,
4

10

, I, I,I,
40

10

-4

- 1 , 1,1,1.
4

100

28.50 (min)
30.
35.
40.
50.
60.
70.00 (max)

RMS %
Error
1.13

o
-u

1 , 1,1,1,
40

100

Kmax (Ksivin)

Kmax (Ksivin)
Kmax (KsiVin)

10

V.

,.1

10

:
10

2
10

-1

10

10

-1

Environment: Water Sat CCI4 10

mfi

+J

X>

10

-Ml 'I'l'l

-L

Environment: Dry CH2I2

(4 of 5)

Kmax (MPaVin)
1

da/dt (10"3in/hour)

Kmax (KsiVin)
29.50 (min)
30.
35.
40.
50.
60.
67.50 (max)

1394
1601.
2163.
2507.
2739.
2740.
2753.

RMS %
Error
20.21

Figure 6.21.3.2.1 (Continued)


6-545

da/dt (10"3in/hour)
926.
933.
1118.
1482.
2779.
4880.
6868.

^ TI-8AI 1 Mo-1V
Condition/Ht:
Form:
Specimen Type: SENT
Orientation:
Yield Strength:
Ult. Strength:

Specimen Thk:
Specimen Width:
Ao:

Kjscc:
Ref: 82651

(5

Kmax (MPaVin)
1

10

b I ' I Tl'l

40

Kmax (MPaVin)

5>

100

1 ' I'l'l'l

-i

10

b I ' I Tl'l

40

100

I ' I M'l'l

- Environment: Water Sat CH2CI2= 1


10

10

10

10

10

10

-J10
\

10

-^10"

\
1 E

.
10

-o
D

-J10

-off
10

^10 i

g
D

110

10

\
1 E
E

-i

z;

-10 >
o

_,

10

10

10

10

10

10

10

10

10

10

I I llll

10

l.l.l,
40

10

100

10

''III

4l0

100

Kmax (KsiViin)

Kmax (KsiVin)
Kmax (KsiVin)

i I i lih

Kmax (KsiVin)

da/dt (10"3in/hour)

RMS %
Error

RMS *
Error

Figure 6.21.3.2.1 (Concluded)


6-546

da/dt (10'3in/hour)

1
Condition/Ht:
Form: 0.13 in. Sheet
Specimen Type: SENT
Orientation:
Yield Strength: 150 ksi
Ult. Strength:

10

- I ' I 'I'l'l

40

QAI
J/-M

IU~

I IVIU

(1 of 1)

Kmax (MPaVin)
1

100

I ' I Tl'l

Environment: 3.5 NaCI

_!
10

_ I

4
10
i I i|i|i|

40
100
i | i|i|i|
-i

10

102

102
10

101

10

101
2 ^

10

|io
\
c

10

10

??
\
1 E

^io"

-M 10
T3

10

>
X)

-2
10

I-

I* T
^^

10

<I>

\
o
~

1\/
I
IV I

Specimen Thk: 0.125 in.


Specimen Width: 3 in.
Ao:
Kiscc: 22 ksi
Ref: 77456

Kmax (MPaVin)
1

T:

\
o
"

4->

10

>
~o

-2
10

-1

10

10

10'3

10"3

-2

10

~ I , I.I,I,

in"*

10

I , I,I,I,
40

" 1 , 1,1,1,

m"4
1

100

10

I , I, I,I,
40

100

Kmax (KsiVin)

Kmax (KsiVin)
Kmax (KsiVin)

-2

10

da/dt (10" 3in/hour)

Kmax (KsiVin)

RMS 5?
Error

RMS %
Error

Figure 6.21.3.2.2
6-547

da/dt (10"3in/hour)

\ Ti-8AI-1Mo-1V r
Condition/Ht: 1520F 1HR WQ
Form: 0.25 in. Plate
Specimen Type: DCB
Orientation:
Yield Strength: 124 ksi
Ult. Strength:
(1

Kmax (MPaVin)
4

10

40

' I 'I'll

Specimen Thk: 0.25 in.


Specimen Width:
Ao:
K]scc*
Ref: 83689

of 6)

(2 of 6)

Kmax (MPaVin)
1

100

- I

' I'l'l'l

10

' I 'I'l'l

40

100

' I 'I'l'l

Environment: Dist. Water; R.T. -=i 10

-Environment: 9MHCI TiCI3; R.T. 10


10

10

10

10
10

10
2

10

10

i-

\
1 E
E

I
I

10
\
c

-1

10

I-

10
10

X)

10
T3

T3

10

10

10

10
10

10
-2

10

10

Al

10
1

10

' i i mi
40

10

'

16.00 (min)
20.
25.
30.
35.
40.
50.
60.00 (max)

10

I I llll

40

100

Kmax (Ksivin)

Kmax (K sivin)
Kmax (Ksivin)

I I I III

100

da /dt (10_3i

Kmax (KsiVin)
26.00 (min)
30.
35.
40.
50.
60.00 (max)

700.
1848.
3569.
5098.
6260.
7104.
8238.
9154.

RMS 55
Error
9.79

RMS 55

Error
22.24

Figure 6.21.3.2.3
6-548

da/dt (10"3in/hour)
96.2
179.
330.
498.
659.
626.

\ Ti-8AI-1Mo-1V h
Condition/Ht: 1520F 1HR WQ
Form: 0.25 in. Plate
Specimen Type: DCB
Orientation:
Yield Strength: 124 ksi
Ult. Strength:

Specimen Thk: 0.25 in.


Specimen Width:
Ao:

KjsccRef: 83689

(3 of 6)

Kmax (MPaVin)
1

b I

10

' I 'I'l'l

40

100

' I'l'l"

Environment: Glycerine; R.T.

(4 of 6)

Kmax (MPaVin)
4

10

t I ' I'l'l'l

40

100

1 ' I 'I'l'l

Environment: HN03; R.T.

-= 1

-=110

10

10

10

10
10

10

10
=5

- I

~ 10"
sz
\
_
c

-^10-3
\
o
x>

-El10 I

3
h10~
\
c

-A A

10

Jio >
XI

^h
10

a
-o

XI

10
-3

10

10

10

10

10

10

Uii

10

10

I I I llll
4
10

10

I I 11 III
40
1 00

26.00 (min)
30.
35.
40.
50.
60.00 (max)

RMS %
Error
18.77

40

1 00

Kmax (Ksivin)

Kmax (Ksivin)
Kmax (KsiVin)

I l.l.l.

da/dt (10~3in/hour)

Kmax (KsiVin)
33.80 (min)
35.
40.
50.
60.00 (max)

1.70
1.87
3.14
5.46
9.93
9.53

RMS %
Error
10.49

Figure 6.21.3.2.3 (Continued)


6-549

da/dt (10"3in/hour)
1.02
1.51
2.45
7.50
7.29

^ TI-8AI1 Mo-1V
Condition/Ht: 1520F 1HR WQ
Form: 0.25 in. Plate
Specimen Type: DCB
Orientation:
Yield Strength: 124 ksi
Ult. Strength:

Specimen Thk: 0.25 in.


Specimen Width:
Ao:
Kjscc:
Ref: 83689

10

40

- I I I'I'l'l

100
a

I ' I 'l'l'l

r^
J

10

10"

""""

~"

-M 10"

100

' I 'I'l'l

10

10
10

10

i-

_c
\

10

V.

-4 A

TO"1 1
10

-J10

>

10

-=Mo

\
o
"

10
T7

-2
10

10

10

III I

10

40

10

10

' I'l'l'l

Environment: Ti CI4; R.T.

10

10"
\

t- I

10

Environment: Methanol; R.T.

(6 of 6)

Kmax (MPaVin)

(5 of 6)

Kmax (MPaVin)

10

10

I . LI,I,

10
4

10

40

Mill
4
10

10

100

12.00 (min)
13.
16.
20.
25.
30.
35.
40.
50.
60.00 (max)

RMS %
Error
26.75

0
40

100

Kmax (Ksivin )

Kmax (KsiVin)
Kmax (KsiVin)

. i I i.n

Kmax (KsiVin)

da/dt (10"3in/hour)

16.80 (min)
20.
25.
30.
35.
40.
50.
60.00 (max)

1.68
5.53
46.2
135.
179.
175.
175.
201.

298.
373.

RMS %
Error
8.49

Figure 6.21.3.2.3 (Concluded)


6-550

da/dt (10"3in/hour)
16.7
21.5
31.6
40.5
44.6
45.4
47.4
115.

Ti8AI-1M01V
Condition/Ht: 1520F 1HR WQ
Form: 0.25 in. Plate
Specimen Type: DCB
Orientation: TL
Yield Strength: 124 ksi
Ult. Strength:
Kmax (MPaVin)
4

10

' I 'I'l'l

40

Specimen Thk: 0.25 in.


Specimen Width: 1 in.
Ac-: 0.985 in.
Kiscc:
Ref: 83689

of 6)

100

1 ' I 'l'l'l

Environment: 5H20/1HCI
-1.9 to -1.5; R.T.

-H

10

(2 of 6)

Kmax (MPaVin)

10

_ I . I llTl

40

100

1 1 lllll,

-1
10
-

-Environment: 5H20/1HCI
_ -1000MV; R.T.
10

10

10
101

10

10

10' I

| 10
\
_

i_

| 10
\
c

>

1-

f
I

^10

-M 10"

\
O

10

10 2

-=

io' I

n "O

-= 10

-n

"O

_, :
-

l-

10

10'

-= 10

10
-3

10
-2

10

LL

' i i i in

10~

10

' 111 HI

40

Ill I

io~:

46.50 (min)
50.
60.
70.00 (max)

RMS %
Error
1.56

I , l.l.l,

10
4

100

10

100

Kmax (Ksivin)
Vm

Kmax (Ksivin)
Kmax (KsiVin)

-= 10

da/dt (10"3in/hour)

Kmax (K sivin)
17.00 (min)
20.
25.
30.
35.
40.
50.
60.
70.00 (max)

4980.
5251.
5848.
5819.

RMS %
Error
40.62

Figure 6.21.3.2.4
6-551

da/dt (10'3in/hour)
168.
903.
3256.
4993.
5561.
5665.
6453.
10102.
22488.

\ Ti-8AI-1Mo-1V F
Condition/Ht: 1520F 1HR WQ
Form: 0.25 in. Plate
Specimen Type: DCB
Orientation: TL
Yield Strength: 124 ksi
Ult. Strength:
(3

Kmax (MPaVin)
1

Specimen Thk: 0.25 in.


Specimen Width: 1 in.
Ac-: 0.985 in.
Kiscc:
Ref: 83689

10

40
100
i i IIIII=n
b I ' I Tl'l


10
- Environment: 5H20/1HCI
_ -400MV; R.T.

_ I

Ti

10

. Pill.)

40

6)

100

1 1 >jllll

-I

- Environment: 5H20/1HCI
_ -200MV; R.T.

10
-

-= 10

10

10
10

iP*

101

101
10

sX

l-

3
O

.c
\

110
\
c
o

(4

Kmax (MPaVin)

6)

10

i E
$=

| io

10

o
X>

-2

10

1-

~
-r:
= 10

E
o

-= 10

" 10-2r

-= 10

Ill I

10

.c

\
c
+, 10"

10

-n 10

-=: 10

-3

-3

10

10

10

i ,I.I.I,

10

10
4

10

4o

100

15.70 (min)
16.
20.
25.
30.
35.
40.
50.
60.
68.00 (max)

40

100

Kmax (KsiVin)

Kmax (KsiViin)
Kmax (KsiVin)

10

Kmax (KsiVin)

da/dt (10"3in/hour)

49.50 (min)
50.
60.
70.00 (max)

190.
225.
1047.
2394.
3328.
3861.
4278.
5633.
9067.
15513.

RMS %
Error
8.89

RMS %
Error
35.81

Figure 6.21.3.2.4 (Continued)


6-552

da/dt (10"3in/hour)
5721.
5869.
15346.
16018.

1 Ti-8AI-1Mo-TVJ
Condition/Ht: 1520F 1HR WQ
Form: 0.25 in. Plate
Specimen Type: DCB
Orientation: T-L
Yield Strength: 124 ksi
Ult. Strength:
(5 of 6)

- I

10

' I 'I'l'l

40

' I 'I'l'l

10

-Environment: 5H20/1HCI
_ +500MV; R.T.

10

= I ' I 'I'l'l

40

100

I ' I 'I'l'l

- Environment: 5H20/1HCI
_ +1000MV; R.T.

_L

10

102

10
10

io3

o
o

-4
10

o,

mn

O,

\
c
^^
^10"3

O,

Jio"

da/dt (in/hour)

"^
2

da/dt (mm/hour)

10-1

"

100
_L

(6 of 6)

Kmax (MPaVin)

da/dt (mm/hour)

Specimen Thk: 0.25 in.


Specimen Width: 1 in.
Ao: 0.985 in.
Kjscc:
Ref: 83689

Kmax (MPaVin)
1

II

io-5

10"3
-4

io"2

10

~~ I , I,LI,

10"8

I , I,I,I,

4
10
40 100
Kmax (KsiVin)

Kmax (KsiVin)
29.00 (min)
30.
35.
40.
50.
60.
63.00 (max)

" I , l.l.l,

10"4

10

I , I,I,I,
40

100

Kmax (KsiVin)

da/dt (10"3in/hour)

Kmax (KsiVin)

0.850
0.871
1.57
3.46
7.48
7.20
7.30

RMS
Error

RMS %
Error
17.47

Figure 6.21.3.2.4 (Concluded)


6-553

da/dt (10"3in/hour)

-\ Ti-8AI-1Mo-1V
Condition/Ht: 1725F FC 1200F 3HR WQ
Form: 0.25 in. Plate
Specimen Type: CB
Orientation: TL
Yield Strength:
Ult. Strength:
f

Kmax (MPaVin)
1

4
=

10

I ' I M'l'l

40

Specimen Thk: 0.25 in.


Specimen Width: 2 in.
Ao: 0.25 in.
Kjscc:
Ref: 85855

100

' I 'I'l'l

- Environment: 21 OOOppm Cl;


_ 32T

(2 of 4)

Kmax (MPaVin)

4)

- |

10

' I 'I'l'l

40

100

' I 'I'l'l

Environment: 21 OOOppm Cl;


72T

-=j10
^
10

10

10

10
10

101

10

I-

v!

110
\
c
-1

10

-a
10

1-

I 10
\
c
-M 10"

T3

10

10

10

10
10

10

-2

10

10
10
4

I III!
10

'

Li

ILI Lli

10

I I I 111

40

100

Kmax (KsiVin)
21.00 (min)
25.
30.
35.
40.
50.
60.
61.00 (max)

10

I.I LU
40

100

Kmax (Ksivin )

Kmax (KsiVin)

RMS %
Error
1.57

"d10
^

Kmax (KsiVin)

da/dt (10"3in/hour)

17.00 (min)
20.
25.
30.
35.
40.
50.
57.00 (max)

2892.
5436.
6567.
7067.
8124.
10376.
11020.
10999.

RMS %
Error
3.32

Figure 6.21.3.2.5
6-554

da/dt (10"3in/hour)
5014.
7759.
11801.
14738.
16734.
18121.
20090.
21366.

^ Ti-8AI-1Mo-1V r
Condition/Ht: 1725F FC 1200F 3HR WQ
Form: 0.25 in. Plate
Specimen Type: CB
Orientation: TL
Yield Strength:
Ult. Strength:
(3 of 4)

Kmax (MPaVin)
1

10

b I ' I'l'l'l

40

Specimen Thk: 0.25 in.


Specimen Width: 2 in.
Ac-: 0.25 in.
Kjscc:
Ref: 85855

100

I ITI'I

- Environment: 21 OOOppm Cl;


140T

(4 of 4)

Kmax (MPaVin)
4

10

40

100

b I ' I M'l'lI ' I M'l'l


Environment: 21 OOOppm Cl;
200T

"d10
^

10
^

10

10

^ D

10
10

10

10

-J10 I

10 2

\
c
-1

-I

10
c

I-

10

-~10
-a
tz

10

-JlO >
10

10

10

10
-3

10

10

10

10

10

I III!

10

10

-L.

40

16.00 (min)
20.
25.
30.
35.
40.
50.
60.00 (max)

10

I I.I.I.
40

100

Kmax (Ksivin )

Kmax (Ksivin)
Kmax (K sivin)

i l ilMi

100

da/dt (10_3in/hour)

Kmax (KsiVin)

7709.
10915.
16530.
23037.
29281.
34200.
37827.
33748.

RMS *
Error

RMS %
Error
7.58

Figure 6.21.3.2.5 (Concluded)


6-555

da/dt (10"3in/hour)

H Ti-8AI-1Mo-1V
Condition/Ht: 1725F FC 1200F 3HR WQ
Form: 0.25 in. Plate
Specimen Type: CB
Orientation: TL
Yield Strength: 150 ksi
Ult. Strength:
Kmax (MPaVin)
1

- I

10

' I 'I'll

40

' I'l'l'l

1
_ I

~= 10
-

4
10
I I llTl

40
100
I I llllll
-I

Environment: 32T:
_ Water 100ppm Cl

-= 10
-

10

10'
_

10

10

10'
2

d**
x: 10

i-

rfP03

10

10

__

10

~10~

T3

-Jio
>

10"

IO

, I,I,I,
40

-2

10

1 , 1,1.1,

10
1

100

10

40

100

Kmax (Ksivin)
<sivin]

Kmax (Ksivin)
Kmax (KsiVin)

10' 1

-1

Ill 1

Ill I

10
10

^
o

10

10

10"

* -a
10 o

.ol-

10

10"

(2 of 4)

Kmax (MPaVin)

of 4)

100

Environment: 32R
_ Water 0.1 ppm Cl
10'

Specimen Thk: 0.25 in.


Specimen Width: 2 in.
Ao: 0.25 in.
Klscc:
Ref: 85855

Kmax (KsiVin)

da/dt (10"3in/hour)

RMS %
Error

RMS %
Error

Figure 6.21.3.2.6
6-556

da/dt (10"3in/hour)

^ Ti-8AI-1Mo-1V r
Condition/Ht: 1725F FC 1200F 3HR WQ
Form: 0.25 in. Plate
Specimen Type: CB
Orientation: TL
Yield Strength: 150 ksi
Ult. Strength:

10

I 'I'l'l

40

100

' I 'I'l'l

Environment: 32T; ,
_ Water 6000ppm Cl

(4 of 4)

Kmax (MPaVin)

(3 of 4)

Kmax (MPaVin)
4

Specimen Thk: 0.25 in.


Specimen Width: 2 in.
Ao: 0.25 in.
Kjscc:
Ref: 85855

="

10

10

10

10

40

I ' I I'l'l
I ' I
Environment: 32F;
Water 20000ppm CI

100

'I'l'l

"_i

z 10

"""

10
10

10

-J10

-J 10

1 E
^

jff***3

""

10

g
3

110

10

-1

-o

-o

_, 10

xi

_,
-2

" 10

" 10

-3

10

10

"

10
I

10

-4

10

' I'll

I I llll

40

100

22.00 (min)
25.
30.
35.
40.
50.
58.00 (max)

I , LI,I,

i , I.I.I,

40

10

-2

100

Kmax (Ksivin)

Kmax (KsiVin)
Kmax (KsiVin)

n T3

10

10

10

1-

^10

10

10

da/dt (10"3in/hour)

Kmax (KsiVin)
16.00 (min)
20.
25.
30.
35.
40.
50.
58.00 (max)

3967.
8666.
11058.
12665.
14599.
15992.
17297.

RMS SB
Error

RMS %
Error

2.56

16.05

Figure 6.21.3.2.6 (Concluded)


6-557

da/dt (10"3in/hour)
2834.
7193.
12129.
15062.
16543.
17415.
19351.
22251.

\ Ti-8AI-1Mo-1V
Condition/Ht: MA
Form: 0.16 in. Sheet
Specimen Type: CCP (max load specified)
Orientation:
Yield Strength: 145 ksi
Uli. Strength:

10

- I 'I 'I'l'l

40

100

I ' I Tl'l

Environment: 3.5 NaCI

of 1)

Kmax (MPaVin)
4

a
10

^~

^~
|

10

110

10

i-

10' |

_.

|
*a 10
-a

__

-1

Ill I

10

10

40

20.80 (min)
25.
29.50 (max)

-2

10

I , I,hi,

10
4

100

10

40

100

Kmax (Ksivin)

Kmax (Ksivin)
Kmax (KsiVin)

10

Ill I

10

I , I, I,I,

->

10

J
10

10

^-

n -a
10

10

-^10

10

100

10

10

10

10

40

10

10

10

I III I-

I III

Kmax (MPaVin)

Specimen Thk: 0.16 in.


Specimen Width: 8 in.
Ao:
Klscc: 21 ksi
Ref: 84290

da/dt (10"3in/hour)

Kmax (KsiVin)

56.1
10876.
26046.

RMS %
Error

RMS %
Error
>100.0

Figure 6.21.3.2.7
6-558

da/dt (10"3in/hour)

H Ti-8AI-1Mo-1V r
Condition/Ht: MA
Form: 0.27 in. Plate
Specimen Type: SENT
Orientation:
Yield Strength:
Ult. Strength:

Specimen Thk: 0.26 in.


Specimen Width: 2 in.
Ao:
Klscc:
Ref: 81741

(1

Kmax (MPaVin)
1

10

= I ' I Tl'l

40

of 1)

Kmax (MPaVin)
4
10
czr-i1 1 1 FTT
1111

100

1 ' I Tl'l

Environment: Distilled Water

40
100
' I ' I'l'l
33
10

-=J 1
10

10

10

10
10

10

^10

10 2

1-

I 10

110

= 10

-1

10

10
T3

-2

10

o
"

-=10 >
-2 ~
10
10

10
-3

-3

10

10

-2

10

10
'

10

I I I III

10

I M.I.
40

10

20.00 (min)
25.
30.
35.
40.
49.00 (max)

LL

i 1 im

10

' 1

40

Lii
100

Kmax (Ksivin)

Kmax (KsiVin)
Kmax (KsiVin)

100

da/dt (10"3in/hour)

Kmax (KsiVin)

10.3
118.
614.
1261.
1543.
1600.

RMS %
Error

RMS %
Error
16.05

Figure 6.21.3.2.8
6-559

da/dt (10"3in/hour)

li-SAl-iMo-lV
u

3
**

W$&
0

tr~

Test
Time
(min)

.1
^3

00
t-

l>

to

o es

HP

t-

WM
<

1-1

::*:**:*:

v:*::::?::::.

+
GO
CO

00

Id

s
J4

8 e
'S * ^

H* -.
M S

J3

wi

a ?.?
**
S~

05

mm
o

00

OC

;::::::C*':-:

<N

m
mm

mm
ll^gj

SSJCOJ

CO

t
:::::

OS
00
CO
eo

CO

(N

CN

CO
OS

<M:

rH

t
i

CO
OS

rH

i
i
i

i
::::::::

ill
s
oc

CN

iiiiii

to

y-ia

to

OS

j'.. :' ::

U3

lO

lO

as

OS

CO sssa*
o
O

CO

IS
CM

:-'::'-.r*:

TH

m
n

oa
o

to

lO
OS

os

1Q

os

os

HI
/-co

eo
CN

CN

OS

00
CN
CO

os
rH

CD
CO

''':M>::
:

i
0
<^

'''.-
>

i
: :::::5::::

ill
10

OS
00

CO

<oc

00

CN

CO

OS
00
CO
CO

CO
OS
l-H

1
1

: :

OS

CO
CO

CN
CO
OS

::

:g
oo

W&i

:::::+::
::::: :

t
i
i

:::::::

1-H

to
OS

to
OS

OS

OS
OS

OS

OS
OS

C6

m lO
CN SS*t*

to
CM

to
CN

OS

CD
CN

OS

CN

r-<

: : : : :7: :

OS
CO
CO
CO

CO

yt

c& .

o >':; ':"P'":':-:

:,.

CO
CO

r?

CO

OS
00

00
CN

to
OS

O!
OS

to
CM

CN

to
CO

*r>
CO

to
CO

OS
OS

CN

to
CN
O

::-|b

IS
CN

<>

to
CN

to
D4
:

to
CN

v>

CJ

to
CN

l-H

<-t

l-H

' V r-t'T"

rH

':l-<

l-H

1-1

l-H

ISjirii*;!

l-H

m
u

C5

03

m
u

i;W

x>:^>

"8p

>
Si

CN

<M

: :3

J=

rri

>:::::'::;>:::

00

E-<
fp
^^afx r^i

SI

::S:*;p3*::::::

lilt s lltl

03

is

Shs

8 ^

03

E-5

"S S
o &
* 0

'S "S

3 3
3
5

**

":

CN

CM

l-H

TH

H?
H

E-i

EH

CO
r-l

CN

lO

iH
i

I--SSS

:^1.-

CO

i-l

>!<

O
l-H

^
CN
to

c
D

rH

6-560

Sip:

1 mmO
rJ

J
H

-1

a.

PH

:-::*::

Tf

CO

1*
- -a
0

0)

^5

O 0

ts

1
$

CN

rH
lO

CO

1I

Itt

p
I

rH

E^

t-r

::::::::-:

CO

CO
r-l

Test
Temp
(F)

L5

mull
o

IH

BQ
O
Q

a o I

0)

O
as

^P

o mm

*:*x*:':'

;i^:i

00

OS
m*t>

OS
00
CD
CO

QD

eo

lliifli

OS

00

CO

l-H

:>:::::

to

;-

CO
OS

:-:>:::: :::
t

r-t

111

!i

CO
CO

01

^^
|||p|
liii

it

3
a,

>>

>>

J-3

^1

i-s
*^
B a

Ti-SAl-lMo-lV

.0

OS
00

|:fP

OS

CN

Ai;Mn,Mi.LMj.......;...;,..:.;.i,n

S^sS*

co

WM
**
00

*i

Test
Time
(min)

Hfl

00

''<&

CN
CO
05
rH

,'TH

:;J

rfl
8

"9 M --*

s3 fi

Sfi
H~

CO
0
CO

OS

on

OS

ao
CD

eo

.''.

J35
:*:*:*Gt-"-v

sslf!?';*'

00

iSi;

>-(

CM
CO
05
rH

mm
**

ao
CN

es
IN

CO

CT>

o>

CN
CD
05
rH

'?[

CN

MM:.,;.,,,,

do

:::-:-:::::::::

illrl

00
CD
CO
CO

<o
so

s
rH

05
00
CO
CO
00
CN
CO
05
rH

::-::-:::

CO
CD
rH

rH

IO
05

mmm

mm
..''oo

i^ill
!!
' .-'^ :
KwKvMvK'X
4-

OS
00
CO
CO
00
CN
CO
05
rH

1
1

M&&&&
::;:::::;:;:i:::::::::
. CO.
CO

^P?3:

i^Rl

SSli^Jg^

:::::::::;:::::::::::::::::

IO

rH

;iy:!:[:|:;:;:;:;:;:;::>:!:>::::::::::::::>::

U~

CN
CO
C5
rH

$
^^ffls^^^

CO
1-1

TO

^-v

es S

t
1
1

X-X-M-X

OS
00
CD
CO
00

^lllllllf

F.;.;.;.].;...;.;.!

tt
^O
lllt|lll

10

w>

::

:
n

11

,l:i::;:

'

10

PSK?

05
01
0

s
gililigl^i

05
05
O

10
CN

illS&ScfllS

in
CN

IO
CN
O

:'-:.. ".-U

^^p^
:

'ji.'' ."'

v..;
:

*?
O

to
CN

T-t :

1-1

IO
05

to

to
O)

OS
05

l>

05
05

O
CN

SSSSfK

lil
to
CM

s
: P-

IO
CN

0
CN

to
CN

io
": CN

IO
CN

4
CJ

rH

rH

JO

iis^s

05

IO
CN

to

W5
05

05

'":0

'

'':*B
<N

' -:

OS
OS

IO
CN

to
CN

IO
CN

:tn
CN

IO
CN

$S"*:B

to

rH

'H

rH

i-ili^^s

X
S
**

3.S
l*~

ft

':''T*

:..':

:'x"x'x x

::::::::::-:-::-:::::-:::::-:::

&

<

:*:#;
SUSP

CQ
0

eft
^

P :-$$5|::W**:
5 -

CQ

r*

c
B
2

51!*

-3
2
rH

a> -a

S 6
P %

CQ
O

rii

E3
O

Id
5

mi
Is

HH

tf
0
0

r-3

ftO
w

EH

as

EH

Hg~

"8 S
0 S

a.

>

fcfc

~s0 -sa
3S

<y

'S*
fi0 a0
OB
6-561

rH

3d

CM
rH

ss

X-X-X-X-X-X-T-X

ip
0
0

cn

PQ
O

m%m%.

CQ
O

1>
S

O >

lllll

* "S
8*

CQ
O

0)

188*5
ri'in'm'

:::::::::-::-:::

rH

PN

3 3
iSBI
c

OS

f?

SSSCS:;:

3 is 3
^0) 2
0

is
1:

Ti-8Al-lMo.lV
h

G5
00
CD
CO
00

t-t

CN
CO
C5

as -w
a

HP

Test
Time
(min)

TH

OS

iiii

lli&jij

1-1

CN
CO
05
r-1

CN
CO
05

'.-:::<N.'-':

.:

i-(

Silili

i
i
i

:v:vX-:->XvX

1-*

::::::*:*>::::

to

CN

liii

Tf
CN

e
05

Ss

;9D||:

CM
CO
05

liiii

i-H

i
I

to
05

CO
8885*81888

i-l

::

:-:'':.:Ji6':"

fcH~

III
HI

<N
O

e*
-..yd---

WS

to
05

151
o

IO
CN

M>

to

to

CN

<N

to
CN

U3

to
CN

wi
:-<N-:

IO
CN

05

IO
CM

os

I mi

"9 >M <-^

to

IO
OS

IO
05

hf|
8

Il^ll
:'

00

Si
';.;: :OD;.:

iiill

mm
r*

1
1

::&i
trt

OS
00
CO
CO
OO
CN
CO
05
r-l

Iscl::
o
CO

::4i

JS:

iS

CN
CO
05

t
:-:-:::+:-:
: : : : :7::::

i
i
i

:::::-:+:

IO
CN

liSi
: ::: :

-*
i-i
CN

05
00
CO
CO
00

o>

i-l

^p;
WM

05
CO
CO
CO
00

^i
l#

05

lips

i
i

CN

r*

00

as

to
CN
O

05
05

05
05

d:

to
0

ll

to

o>

OS
05

fi

as

O"

to
CN

to

to
CN

to
CN

*o

to
CN

to
<N

M5
*3

to
OS

05
OS

^i

to
CN

<N :

IO
CN

9tO :
tW.^S

Alii

i-l

I-l

'*

r-l

iH

r-f

1-H

JS?rs

iH

rl

t-l

CO

c$

U5

is^si?

li|:|S

&
tt

<N

::::-::-:-:
Kv:;:;!;:;:;

#:::::::::
588SSK
to

OS

IO

li^li
^s^

i"'
SitSS

CO

SS05.S

111

fK

IO
OS

; y

to

00

:S:*::

IIS

'WjB

;::;:;:S:;:;:
x>:-:::::::

eo
oo

05
00
CO
CO
00

''%::"

;!;!;!;!;!;!:!;!;!;!;!;!:!:!;

OS
00
CO

1II

00

::&'':

t->
CM

ASA

00

i
i

en

sil

H ,3

eo

llllsll

i?

08

OS
00
CO

*;&

PQ
O

m
a

lllfltl
O

m
o

S3
:W^i5::::::::;

m iptl m IB a
o **w* o C^ u
Q p p u
:

03

o
p

:::::::::::-::

~3

'- ST
^^
a> a>

IN

CO CO

::

: : :*IW*::V>

r
u
0) o

Sfc

8
*

cd CN

S.S

#3.
5

Iff

yjlf

111!

**&
*-%

Test
Temp
(F)

^1
H?
rt
1

-o

S
o C

CU

J*
CU fc

US
o a

C
o

or T3C

1*

C a
o a

OS

6-562

> 'C

ll
lllllll

cs

to
CO

-*

s?
J2

CO

o
m
P

: -C
O :
*=>

Ml
<

11

CN

CN

CN

CN

CN

J
H

iJ

fcH

EH

EH

J
fr^

CN
CN

I-l

CD
CO

I-I

CO

"*

to

Ti-8Al-lMo-lV
o

05
00
CO
CO
CO

.8

3
9

0)

rS 8

i-l

Test
Time
(min)

HO

CM
CO
03

i
i

IP
m
CO

CM

';''.*^.
:::::>:::j::::

^^
c

OS
CO
CO
CO
CO
<N
CO
03
H

!;|:|;!;!:j:!:!:
CO
CM

-^,
iiSS**
00

mm
<-<

os

OS
CO
CO
CO
CO

CO
CO
CO
00

CM
CO
OS

|l
$

CM
CO

iH

iiiPiii

;?&$

:-:-:-:-:::fc:$

1
1
1

y'' t " ,.

CD

:-:-:-::>:::

tik&kk

os

I-l

SS:S5:
OS
CO
CM

JO _

54,0s
O
O
w

sissB*;*?:

os

ssS;;

os SS:*:::

as

os
os
o

mm

OS
OS

os

Ui
CM

ssajs

in

in
CM

to

lO
CM
O

\:.:ci!"<?3
o

s?s?*s

OJ
. VO

to
CM

teO

CM

1Q
CM

HO

HJ

CM
O

lO

OS

to
CM

'tb
CM

lO
CM

1
::-:-:-::-:-

:-::ft::::

CO
'
CM

to
as

lO

:8:
.:\,rt

CM
CO

as
T-t

M
m

05
Z

<t>

%m

1-4

00
OS
rH

*H

1
:::::>::

SJS:S

in
mm

.;: as

OS
CO
CD
CO
00

lUi:

lO

:.

CM
CM

CO

CO
CM

W8&

i;s?;
os ssfts

in
OS

in
os

OS
OS

II

OS
OS

i
i

;.;

O
CM

to
CM

to
-*i
;:

lO
CM

ma
o

to
CM

in

in

CM

CM

CM

sn

iH

CO
CO
00

to
CM

1
1

o
a
P.
CO

~
fab
CB
O

tN

CO

I
1

11

43

CO

::-:-::::

lO
OS

'.:.-w .

CM
CO
OS
iH

mm

CM
CM

OS
00
CO
CO
CO

CM

OS

2S s

CM

"2 * o

CO

CO
<N

as

m
m

,yy:-:<yyy.

03

:::-:^3:::

BB
mm
o.

:::

to

: : !C3:::

n
u
Q

W
A

a
u

oa
u
Q

EH

::

:::.^ :

ll Hi!
1 lil
0)

2
a o
.5 *H

ill

32

Vi
2
a
a
CM
+

iff;

as
C

Ill 3s-

3 3g

o >

2 L
k2

tt
O
Q

6
p

m
o

:*:*:-:-::>:-:-:

m
o

: O

:::<*-:

:::***::
::-:>'**:

u
a>
s

TO

si

ii

to
w

OS

* 2

<*

** I

CM

<N

CM

CM

iH

CM
rH

CM

i-H

I-H

i-l

iH

hJ

J
EH

KJ

EH

EH

EH

EH

EH

CO

in

CM

to

CM

EH

<N c

1-H

tt

S;

J2

^1

EH

safe

r2

OS

^1

i-l

ng ~
g

o C

"a-8
o

1*
1

lO

CM

CM

i-l

CM

CO
CM

iH

rf

05

CM

,*.

<y2

^^
S &

Jfe

CM

fa g < feu
to ^ j: <=>
f~ 0 00

o e
OK

iH <3

6-563

iH

Ti-8Ai-tMo-lV

I
to
IO
oo

to
to
oo
IO
00

eo
05

Hfl

|sg;|

I1

Skos

IO
IO
CO

to
oo

IO
00

eo

IP

t05

: 00 i

eo
t>

05

to
to
oo
to

00

eo

CO

05

OS

8 S -5

All
CO

SO;

es

IO
CS

IO

es
d

;;.<o.:

es
d

CS

S ti

CO

:**$?;

eo
CO
IO

CO

JA

"O JA ^

If

CO

so*:'
o

es

U3

to

:'.<

;:..;;

SSlS

SS9

K*OS

IO
OS

ip

mm

ca-.-i

es

CO

: <N

f'-CD

mm

to

IO
CS

CM

cvi

es
d

e
IN

d
to

eo

: CO

es
:

: u5 :

Si

to
es

o
CO
00

IO

es

ft
GO

EH

LE*.;
00

Hi
2 .a
cog

05

fa

s
g
es
SO

fa
fa

fa
&|

II

tell

fa

2c

rH O
ess

"O

fe 2
SO

;;

55
#
IO
CO

IO

kO

to

EH

EH

EH

EH

EH

EH

es
CO

EH

EH

EH

fa

fa

fa

fa

es

tf
02I

GO

as

g Bfe

EH

ft5

es

fa

cu fa

"ao -s

I*
5 *
O

ffi

OB

fa
e
TH

,
fa <N
o TH
O

1H

cy

O es

S fa fa o
fa rj
iJ -c
eo

fo fa
"-
- ^u fa
~ H. C

SP a<
c h
c- js es es o
H ifl H H
cq

<

6-564

fa3
^

2 > io

Ti-8Al-lMo-lV
fa
<s

.0

;.;.;-:^K;-:
K-yufi*

5
Test
Time
(min)

HQ

^^

s
S~
&
8

PP
IK

ffi&

t~
CN

t~
CN

t~
CN

"
00

00

><*<

eo

t~
CD
Oi
rH

-:::::+:::

eo

f-

co
0)
rH

t~
CM

eo

eo

S1

t~
CN

tCN

**

T)<

eo

eo

t~
CN

eo

"#

00

CO

CO

CO

CO

t~
CO

tCO

t-

r-

tCO

rH

T-i

rH

en

en

1
t

I
I

1
1
1

co
en

1
1

CO
CO

rH

en

1-1

:v:;::i:

m
*

CO

*-

'S
es 6

CO

en

- T*

1-4

1
1
1

53

0
0)

a
^w

ft

lil

00

eo

rH
CO

rH

rH

-*

CO

OS

eo

r*
<a

to

10

CO
CO

eo

eo

eo

CO

CO

CO

to
mam

eo

CN
CN

IO
to
10

:fflr::;

rH
0

to
CN

10

to

CN

Ifl

lO

U V.

EH

*|

'6

3 fa -a
W
L2

05

*0 cS
fa 0

0 0

1*
1
0 0

OB

rH

rH

rH

*H

EH

ij
U

.;

:::::+::: :::::+::
3

r:.W.

CO

to

<J> mm s:o|

: : : : :+:::-

'*:.
t

;::::

: : : : :+::::

CO
CD

00
CO

rH

rH

to
to
CN SSS&
^ ssSS?
r
SS?*:;:

00: >}gB:;:

MP
%
1
H
TH
op

en

en

1
1
1

:::::-:::

*
CO

CO

CO
OJ

10
CO

*
TT

to
CO

CO

CO

Q ..-:o

;o

11P1

EH

2
03

eo
CJ

^
10

)ri

lit
ftii ill ill;
'

*
iiiiii^P
mmwmtz

0)

*o
to

10

rH

rH

eo

03

iJ

EH

EH

E
C

EH

CU

03

PH

>-

0)

O CO

3 "3 fe O
'S Si 0 fc

i3
'Sa

^3

6-565

EH

m&

to

;;'.

to

ti

j I
U | Uli;:

eo

rH

<>

"EH

eo

ii;

*EH

03
EH

03
J

raWJ

.;j^^.>^^

eo

I-.

tCN

CN
O

S5

10

'.

:-:::-:]:-:

ii**
S*K

CN
rH

1
1

10
CN

CD
-VrH.'

eo

a
2
*
10

to
0

eo
ca

e>

-:-:::-::::-:-:-:-:

>
25

Test
Temp
(F)

tt

'?

5S

::::>::

: :: : :

<S0

**

S^S

00

;*S*S

OS

CO
CN
CO
^f
CO

CO

:!:S:;S;;|
::$?::
::::-::::

to

:iB c
ill
mm TH rH

CD

Prod
Thk
(in)

to

PSs

S
J<J

to

sss^ft ssfel* CN
roea*
CO
*
eo
co
^s
^
t**
**
00
00
00
t-

to

' '

ss$si!i

'S

> cF

wsmsm
mmmmz

Ti-8Al-tMo-lV

J
<o
mmxtmm

u
S

1111111
.-.:. 03

iltllpli
,

: K >KVK^S *:'HV:V

::::::;:>:ft3K:::-:ft

Hfl

Test
Time
(min)

4i a
00 +
9 03

^:::::::::^^:3:S
::::::::-:-:->::::::::
:>:':'ft":vft>>:::::::::v

^**
a

il

>^s

fi

.tt

o o
s S
fc<

llAl

"5^/-.
22 ^

"* ^
S c
5
H

c0

s
u

t-*
D5
O

e
>
o

*fi
!SW

as

\i;;-T-*::

&

Iltltil

*^

P4

:>KWK<<::::&W.:.V.

to

lillllll

a
' ''S .:-.; .-

P4

^S$8
1

Ilglp
: :- i22;:.-

S
2

a
&

ao

::

o
00

2ta

uS
CO

""i

8
e
S

e
&

^^

o
+
0

"O
S
0 s

fi

&

00

0D

*1

0
0

e
C

1
** 0

o
o

B
g
ft

00

"o "8o

1*
1

0 0

oa

a> ,-.

> Si

a
6-566

Ti-Mo8V2Fe3Al

H>

CO

,
2 a

a s
X

co

p
0
0
o

.5
o

J
FH

tf

"

JQ

f-i

a
. S

05
CO
lO

CO

CO

H
>J
CM

0 >

Co a

19

CD

w
fl
V

*
03
O
h

-u
cd

OS

S
CO
fa
O

l-H

EM

<

Ed

'S

<
Ed
OS

<
fco

u
w

" fc

0
P
Cfa

a
EL,

PH

6-567

\ Ti-Mo8V2Fe3Al

BS

I
is
tf

2
O

55
w

15
N
CO

J8

i*

9es
Hg

BS

BS

a
a.

s
BS
S

to
b

a
a

C
H

H
BS

K
BS

to oo

o
i- Of

6-568

Ti-5A12.5Sn ELI

I
5>
SB

ISE"3

*4

m
w

w
a

goB to

03
CO

a
65

a.

as

i*

S
3

9n

"7
a
o

'$

!
Z

<

D
ar
a

6-569

Ti-5A12.5Sn

miii

t^E

rfi

5*<

S3
tf

z
a

3 o

l-S*

a. o

6^

E
o

I
o

6-570

Ti-6A!6V2Sn ELI i

iJ
CO

c
03

CO Q

"8 >
COD

s
fl
o
**
o

'S

tg

3
o

a
S
"5

.u

tf

a>

CG

H
H4

CO

CN

oj

lO

lO
CO

coe
c

00
oj

03

PS

OS

CO

fl

0>

2
&

-w

es

<

<

X
Ex.
o

Ex.
o
IS

U5

o
l-H

fH

Of

0)

HM

rH

-I

Eh
O

Ec
O
o

co

t-t

u
-w

s a

" is
o o
u fa

o
a!
CH

&

6-571

Ti-6Al6V2Sn ELI

5H

feo

M
rfi

1
si-
<.**
a

w
05

s "2 (0

Ed

CO

a.
as

J8

S*

3pi
CO

BSf?

E-

E"

E-

cd

a
o

<
s

8
B
S3

<

03

a.

6.

8
9

S3

6-572

as

TABLE 6.25
KEFERENCES FOR THE TITANIUM ALLOY DATA

54304

Ti-6A1-4V

K,

Figge, I. E., "Residual Static Strength of Several Titanium and Stainless Steel Alloys
and One Superalloy at -109 F, 70 F, and 550F," NASA TN D-2045, Langley Research
Center (December 1963).

57573

Ti-6A1-4V

Anon., "Fracture Toughness and Tear Tests," Air Force Materials Laboratory, Research
and Technology Division, Report No. ML-TDR-64-238, October 1964.
58782

Ti-6A1-4V

K.

Anon., "Thick Section Fracture Toughness," ML-TDR-64-236, Boeing-North American


(October 1964).
60578

Ti-6A1-4V ELI

K;

Christian, J. L., Yang, C. T., and Witzell, W. E., "Physical and Mechanical Properties
of Pressure Vessel Materials for Application in a Cryogenic Environment,"
ASD-TDR-62-258, Part III, General Dynamics/Astronautics (December 1964).
66103

Ti-5Al-2.5Sn

K,

Ferguson, C. W., "Hypervelocity Impact Effects on Liquid Hydrogen Tanks," NASA


CR-54852, Douglas Aircraft Co., Inc. (March 1966).
66218

Ti-5Al-2.5Sn

K,

Tiffany, C. F., Lorenz, P. M., and Hall, L. R., "Investigation of Plane-Strain Flaw
Growth in Thick-Walled Tanks," NASA CR-54837, The Boeing Company,
(February 1966).
67821

Ti-8Al-lMo-lV

K,

Walker, E. K., "A Study of the Influence of Geometry on the Strength of Fatigue
Cracked Panels," AFFDL-TR-66-92, Northrop Norair (June 1966).

6-573

TABLE 6.25 (CONTINUED)


REFERENCES FOR THE TITANIUM ALLOY DATA

68968

Ti-5Al-2.5Sn

K,

Sullivan, T. L., "Uniaxial and Biaxial Fracture Toughness of Extra-Low-Interstitial


5Al-2.5Sn Titanium Alloy Sheet at 20 K," NASA TN D-4016, Lewis Research Center,
(June 1967).
70733

Ti-8Al-lMo-lV

K^,

Smith, H. R., et al., "A Study of Stress Corrosion Cracking by Wedge-Force Loading,"
Report D6-19768, The Boeing Company, Renton, Wash., Contract N00014-66-C-0365,
(June 1967).
70887

Ti-6A1-4V
Ti-6Al-6V-2.5Sn
Ti-8Al-lMo-lV

K^
K^
Kisa

Peterson, M. H., Brown, B. F., Newbegin, R. L., and Groover, R. E., "Stress Corrosion
Cracking of High Strength Steels and Titanium Alloys in Chloride Solutions at
Ambient Temperature," Corrosion, 23 (5), 142-148 (May 1967).
70931

Ti-6A1-4V
T1-6A1-4V ELI
Ti-6Al-6V-2.5Sn
Ti-8Al-lMo-lV

K^,
K^
K^
K^,

Judy, Jr., R. W., and Goode, R. J., "Stress-Corrosion Cracking Characteristics of Alloys
of Titanium in Salt Water," Interim Report 6564, Naval Research Laboratory,
Washington, D. C, Contracts NONR-610(09), NONR-760(31) and N00014-66-C0365
(July 21, 1967).
71709

Ti-8Al-lMo-lV

K,

Figge, I. E., "Residual-Static-Strength and Slow-Crack-Growth Behavior of


Duplex-Annealed Ti-8Al-lMo-lV Sheet," NASATN D-4358, Langley Research Center,
(March 1968).
74355

Ti-6A1-4V

Kj,,

Stanley, J. K, "Solutions to Some Stress Corrosion Cracking Problems in Aerospace


Applications," Technical Report TR-0200 (4112.22)-1, Aerospace Corporation, El
Segundo, Calif., Contract F04701-68-C-0200 (November 1968).

6-574

TABLE 6.25 (CONTINUED)


REFERENCES FOR THE TITANIUM ALLOY DATA

75386

Ti-4Al-3Mo-lV
T1-6A1-4V
Ti-8Al-lMo-lV

K^
Kfe
K^

Curtis, R E., et al., "Relationship Between Composition, Micro-structure, and Stress


Corrosion Cracking (In Salt Solution) In Titanium Alloys," ASM Transactions
Quarterly, 62 (2), 457-469 (June 1969).
75528

Ti-6A1-4V

Kfc

Bixler, W. D., "Fracture Characteristics of 6A1-4V Titanium Alloy Forgings Containing


Alpha Stringer Microstructure," NASA Final Report CR-99512, The Boeing Company,
Seattle, Wash., Contract NAS-9-8809 (January 1969).
76411

Ti-6A1-4V

K*

Wessel, E. T., et al., "Engineering Methods for the Design and Selection of Materials
Against Fracture," Final Technical Report, Westinghouse Research Laboratories,
Pittsburgh, PA., Contract DA-30-069-AMC-602 (T) (June 24, 1966).

77290

Ti-6A1-4V

Kfc

Reuter, W. G., et al., "Monitoring of Crack Growth on Ti-6A1-4V Alloy by the Stress
Wave Analysis Technique," NASA Report CR-101888, Aerojet General Corporation,
Sacramento, Calif. (December 1968).
77456

BETA
BETA Ti
Ti-8Al-lMo-lV

Ki8M
da/dt
da/dt; Kja

Katz, Y., "Micro-Mechanical Approach to Stress Corrosion Cracking in Titanium


Alloys," Thesis Report No. UCRL-19046, University of California, Lawrence Radiation
Laboratory, Berkeley, Calif., AEC Contract W-7405-eng-48 (September 1969).
78535

Ti-6A1-4V

Kj,

Masters, J. N., et al., "Fracture and Nitrogen Tetroxide/Sustained Load Flaw Growth
in 6A1-4V Titanium," Final Report D2-121397-1, NASA CR-109366, The Boeing
Company, Seattle, Wash., Contract NAS7-100 (October 1969).

6-575

TABLE 6.25 (CONTINUED)


REFERENCES FOR THE TITANIUM ALLOY DATA

80104

Ti-5Al-2.5Sn

K,

Orange, T. W., Sullivan, T. L., and Calfo, F. D., "Fracture of Thin Sections Containing
Through and Part-Through Cracks," NASA TN D-6305, Lewis Research Center
(April 1971).
80538

Ti-6A1-4V

Kjc

Petrak, G. J., "Mechanical Property Evaluation of Beta Forged Ti-6A1-4V,"


Report AFML-TR-70-291, University of Dayton Research Institute, Dayton, Ohio,
Contract F33615-69-C-1471 (January 1971).
81221

Ti-6A1-4V

da/dt; K,8CC

Beck, T. R., et al., "Stress Corrosion Cracking of Titanium Alloys: Studies of Cracks
in Thin Specimens; SCC of Ti-6A1-4V in Chloride, Iodide and Fluoride Solutions; Stress
Corrosion Cracking in Molten Salts; Electrochemistry of Freshly Generated Titanium
Surfaces," Report 20, The Boeing Company, Seattle, Wash., Contract NAS 7-489,
(June 1971).
81741

Ti-8Al-lMo-lV

da/dt

Bucci, R. J., and Paris, P. C, "Observations on Sustained Load Environmental Crack


Growth of Titanium 8AI-IM0-IV Alloy," Corrosion, 27 (12) 525-530 (December 1971).

82651

BETA
BETA III
Ti-8Al-lMo-lV

K^
da/dt; Kj.
da/dt

Beck, T. R., and Blackburn, M. J., "Stress Corrosion Cracking of Titanium Alloys; SCC
Velocity; Concentration of TiCl3," Report 18, The Boeing Company, Seattle, Wash.,
Contract NAS 7-489 (December 1970).
83222

Ti-6Al-6V-2Sn

Kjc

Amateau, M. F., et al, "F-15 Program Final Report Ti-6Al-6V-2Sn and Ti-6A1-4V
Fatigue Crack Propagation," Report No. ATR-72(9990)-3, The Aerospace Corporation,
El Segundo, Calif. (September 29, 1971).

6-576

TABLE 6.25 (CONTINUED)


REFERENCES FOR THE TITANIUM ALLOY DATA

83689

Ti-8Al-lMo-lV

da/dt; Kjs

Beck, T. R., et al., "Fundamental Investigation of Stress Corrosion Cracking,"


Report D180-15006-1, The Boeing Company, Aerospace Group, Seattle, Washington,
Contract NASW-2245 (April 1962).
83984

Ti-6A1-4V

K,

Feddersen, C. E, and Hyler, W. S., "Fracture and Fatigue-Crack-Propagation


Characteristics of 1/4-Inch Mill-Annealed Ti-6A1-4V Titanium Alloy Plate,"
Report G-9706, Battelle, Columbus Laboratories, Columbus, Ohio,
Contract N00156-70-C-1336 (November 1, 1971).
84036

Ti-6A1-4V

K^

Beachem, C. D., and Meyn, D. A, "The Effect of Thickness Upon Sustained Load Crack
Propagation in Ti-6A1-4V Alloy Tested in 3.5% NaCl Solution," NRL Report 7449,
Naval Research Laboratory, Washington, D. C. (August 8, 1972).

84282

Ti-6A1-4V

K^

Spurr, W. F., "SST Technology Follow-On Program, Phase I, Titanium Alloy 6A1-4V
Extrusion," Report No. FAA-SS-72-06, Boeing Report D6-60206, The Boeing Company,
Commercial Airplane Group, Seattle, Wash., Contract No. DOT-FA-SS-71-12,
(July 1972).
84290

Ti-8Al-lMo-lV

da/dt

Smith, H. R., Piper, D. E., and Downey, F. K, "A Study of Stress-Corrosion Cracking
by Wedge Force Loading," Engineering Fracture Mechanics, 1, p 123-128 (1968),
Pergamon Press.
84306

Ti-6A1-4V

KIc

Harrigan, M. J., "B-l Fracture Mechanics Data for Air Force Handbook Usage,"
Report TFD-72-501, North American Rockwell, Los Angeles Division, Los Angeles, CA
(April 21, 1972).
84316

Ti-6Al-6V-2Sn
Ti6A16V2Sn ELI

Kjc
K^

DeSisto, T. S., and Hickey, Jr., C. F., "Low-Temperature Mechanical Properties and
Fracture Toughness of Ti-6Al-6V-2Sn," ASTM Proceedings, 65, 641-653 (1965).
6-577

TABLE 6.25 (CONTINUED)


REFERENCES FOR THE TITANIUM ALLOY DATA

84326

Ti-8Al-lMo-lV

Kj,

Report of NRL Progress, Naval Research Laboratory, Washington, D. C, (May 1968).


84327

Ti-8Al-lMo-lV

Kj

Report of NRL Progress, Naval Research Laboratory, Washington, D. C, (May 1967).

84328

Ti-6A1-4V

K^

Report of NRL Progress, Naval Research Laboratory, Washington, D. C,


(November 1968).
84360

Ti-6A1-4V
Ti-6Al-6V-2.5Sn
Ti-6Al-6V-2Sn

Kje; da/dN; da/dt; KIscc


K^
K^; da/dN; da/dt

McDonnell Aircraft Company, McDonnell Douglas Corp., St. Louis, Mo., Phase B Test
Program, Report MDC A0913 (May 18, 1971).
85034

Ti-6A1-4V

K^

Mitchell, John, "Laboratory Reports on Fracture Toughness Tests," per memo from Ed
Cawthorne of February 5, 1973; data sheets from Schultz Steel Co., South Gate, CA.
85064

Ti-6A1-4V

K^

Bjeletich, J. G., "Development of Engineering Data on Thick-Section


Electron-Beam-Welded Titanium," Report N-LJ-71-18, Lockheed Aircraft Corporation,
Lockheed Palo Alto Research Laboratory, Palo Alto, Calif., Contract F33615-71-C-1338,
(October 12, 1972).
85634

Ti-6A1-4V

Kjc

"Fracture Toughness and Tensile Properties Data for Ti-6A1-4V Forgings," Schultz
Steel Company, South Gate, Calif., Attached to memo from Ed Cawthorne dated
March 5, 1973.
85836

Ti-6A1-4V

Kjc

"B-l Fracture Toughness Data (Kjc) - Rockwell International," Rockwell International


Corporation, Los Angeles, CA (April 24, 1973).
6-578

TABLE 6.25 (CONTINUED)


REFERENCES FOR THE TITANIUM ALLOY DATA

85837

Ti-6A1-4V

a-vs-N; da/dN

"Fracture Toughness Data Collection, Rockwell International Corporation, from B-l


Program," Rockwell International Corporation, Los Angeles, CA., April 1973.
85855

Ti-8Al-lMo-lV

da/dt; Kj.

Boyd, J. D., "Stress-Corrosion Cracking of Ti-8Al-lMo-lV in Aqueous Environments:


1. The Kinetics of Subcritical Crack Propagation," Metallurgical Transactions, 4 (4)
1029-1035 (April 1973).
85857

Ti-6A1-4V

Kjc

"Shultz Steel Company - Fracture Toughness Data - May 10, 1973," per memo from
Ed Cawthorne of May 10, 1973.
86099

Ti-8Al-lMo-lV

a-vs-N; da/dN

Wanhill, R. J. H., "A Review and Analysis of Fatigue Crack Propagation in Titanium
Alloys at Room Temperature," Report No. NRL-TR-71035U, National Aerospace
Laboratory, The Netherlands (February 1971).
86429

Ti-Mo8V2Fe3Al

Kj,

"Fracture Toughness Data," Progress Report on Materials Test Program, General


Dynamics Corporation, Fort Worth Division, Fort Worth, Texas,
Contract F33615-72-C-2149 (Received July 6, 1973).
86494

Ti-6Al-6V-2Sn

Kj,

Harmsworth, C. L., "Evaluation Report - Fracture Toughness Evaluation of


Isothermally Forged Ti-6Al-6V-2Sn STA," Report MXE 72-64, Air Force Materials
Laboratory, WPAFB, Ohio (November 15, 1972).
86575

Ti-6A1-4V

a-vs-N; da/dN

"Rockwell International, B-l Program, da/dN Data, Center-Cracked Tension


Specimens," Lockheed California Company, Burbank, CA, Report LR25152
(Received July 1973) (Memo from Ed Cawthorne dated July 10, 1973).

6-579

TABLE 6.25 (CONTINUED)


REFERENCES FOR THE TITANIUM ALLOY DATA

86688

Ti-6A1-4V

K*; Kj,

Sprowls, D. 0., et al., "Evaluation of Stress Corrosion Cracking Susceptibility Using


Fracture Mechanics Techniques," Final Report Part I, Aluminum Co. of America, Alcoa
Technical Center, Alcoa, Pa., Contract NASA-21487, May 31, 1973.
86844

Ti-6-2-2-2-2
Ti-6Al-6V-2Sn

a-vs-N; da/dN
a-vs-N; da/dN

"Crack Growth Rate Data Generated Under USAF Contract F33615-72-C-2165,"


Lockheed Aircraft Corporation, Lockheed-Georgia Company, Marietta, GA,
Contract F33615-72-C-2165, Data Sheets received from AFFDL August 13, 1973.
87230

BETA III
Ti-6Al-6V-2Sn
Ti-Mo8V2Fe3Al

K^
Kjc
Kjc

DeSisto, T. S., "Fracture Toughness Measurements of Three Titanium Alloy


Extrusions," Report AMMRC-TR-73-31, Army Materials and Mechanics Research
Center, Watertown, MA (July 1973).
88140

Ti-6A1-4V
Ti-6A1-4V EU

da/dN
da/dN

Hall, L. R., Finger, R. W., and Spurr, W. F., "Corrosion Fatigue Crack Growth in
Aircraft Structural Materials," Report AFML-TR-73-204, Boeing Aerospace Company,
Seattle, WA. Contract AF33615-71-C-1687 (September 1973).
88144

BETA III
Ti-6A1-4V

K^; da/dN
K,c; da/dN; da/dt

Bjeletich, J. G, "Development of Engineering Data in Thick-Section Electron Beam


Welded Titanium," Report AFML-TR-73-197, Lockheed Missiles and Space Company,
Inc., Palo Alto, GA, Contract F33615-71-C-1338 (August 1973).
88186

TI-*
Ti-6Al-6V-2Sn

Kfc
K^

"Selected Pages from Materials Section of Final Report on Cargo/Tanker Phase IA


(AFFDL-TR-73-51) Lockheed Report SMN 378," Summary Report, Lockheed-Georgia
Company, Marietta, GA, Contract F33615-72-C-2165 (February 8, 1974).

6-580

TABLE 6.25 (CONTINUED)


REFERENCES FOR THE TITANIUM ALLOY DATA

88439

Ti5A12.5Sn ELI

Kfc

Reuter, W. G., "Fracture Toughness of Ti-5Al-2.5Sn ELI Forgings at -423 F,"


Summary Report, Aerojet-General Corporation, Sacramento, CA (September 9,1970).

88440

Ti-6A1-4V

Kfc

"Titanium-6A1-4V Fracture Toughness and Tensile Test Data of December 19, 1973,"
Memo E. W. Cawthorne with fracture toughness data from Schultz Steel Company
(December 19, 1973).

88468

Ti-6A1-4V

a-vs-N; da/dN

Bell, P. D., "Data Sheets for Constant Amplitude Crack Growth Data Generated by
Grumman Aerospace Corporation for 2219-T851 Aluminum and Mill Annealed 6A1-4V
Titanium Alloy Plate," letter to J. E. Campbell from Grumman Aerospace Corporation,
Bethpage, NY, Contract F33615-72-C-1744 (March 15, 1974).

88575

BETAC
Ti-6A1-4V

Kjc; a-vs-N; da/dN


Krc; a-vs-N; da/dN

"Advanced Metallic Air Vehicle Structure Program," Material Property Data Test
Report Phase II, Report FZM-6148A General Dynamics, Convair Aerospace Division,
Fort Worth, TX, Contract AF33615-73-C-3001 (January 1974).

88579

Ti-6A1-4V

a-vs-N; da/dN

"B-l Program da/dN Data for Aluminum Alloys," Rockwell International Corporation,
memorandum to H. D. Moran from E. W. Cawthorne, Battelle's Columbus Laboratories
(April 3, 1974).

88700

Ti-6A1-4V

Kfc,

Gilbreath, W. P., and Adamson, M. J., "The Stress Corrosion Susceptibility of Several
Alloys in Hydrazine Fuels," NASA Technical Note, Report NASA TN D-7604,
Ames Research Center, Moffett Field, CA (February 1974).

88911

Ti-5Al-2.5Sn

a-vs-N; da/dN

Wanhill, R. J. H., et al., "Fatigue Crack Propagation Data for Titanium Sheet Alloys
- Interim Report No. 3:Ti-5Al-2.5Sn," Report NLR TR 72093 U, National Aerospace
Laboratory, the Netherlands (July 1972).

6-581

TABLE 6.25 (CONTINUED)


REFERENCES FOR THE TITANIUM ALLOY DATA

88962

Ti-6A1-4V
Ti-6Al-6V-2Sn
Ti-6A12Sn4Zr6Mo

K*
Kjc
Kjc

Sparks, R. B., and Long, J. R., "Improvement Manufacturing Methods for Producing
High Integrity More Reliable Titanium Forgings," Report AFML-TR-73-301,
Wyman-Gordon Company, Worchester, MA, Contract AF33615-71-C-1560
(February 1974).
89004

Ti-6A1-4V

K,c; Kj.

"Rockwell International, B-l Program Titanium K^, K,, and Kj. Data for HB-01
Revision," with data attached to memorandum from E. W. Cawthorne to H. D. Moran
(May 1, 1974).
89504

Ti-6A1-4V

K^

Cervay, R. R., "Mechanical Properties of Ti-6A1-4V Annealed Forgings,"


Report AFML-TR-74-49, University of Dayton Research Institute, Dayton, OH,
Contract F33615-72-C-1282 (March 1974).
90012

Ti-6A1-4V

K^

"Ti-6A1-4V Fracture Toughness Data - Shultz Steel Company, South Gate, CA, of
August 8, 1974," with memorandum from E. W. Cawthorne to H. D. Moran of
Battelle's Columbus Laboratories (August 8, 1974).
90584

Ti-6A1-4V
Ti-6Al-6V-2Sn

Kjc
Kjc

DeMay, S., "Improved Fracture Toughness of Titanium," Final Report, Grumman


Aerospace Corporation, Bethpage, NY, Contract N62269-73-C-0127 (June 1973)
(AD 778 652).
90589

Ti-6Al-6V-2Sn

Kjc

Fiftal, C. F., and Beck, E. J., "Development of Fracture Mechanics Data for 6Al-6V-2Sn
Titanium Alloy," Report MCR-74-43, Martin Marietta Corp., Denver Division, Denver,
CO, Contract NAS 9-13599 (January 1974).

6-582

TABLE 6.25 (CONTINUED)


REFERENCES FOR THE TITANIUM ALLOY DATA

90981

Ti-6A1-4V
Ti-6Al-6V-2Sn

a-vs-N; da/dN
K*; a-vs-N; da/dN

Krupp, W. E., Wimmer, F. T., Pettit, D. E., and Hoeppner, D. W., Data Sheets for
Final Report on "Investigation of the Effects of Stress and Chemical Environments on
the Prediction of Fracture in Aircraft Structural Materials," Rye Canyon Research
Laboratory, Lockheed-California Company, Burbank, CA, Contract F33615-71-C-1688,
data sheets received October 21, 1974.
91332

Ti-6A1-4V

da/dN

Wells, R. R., "New Alloys for Advanced Metallic Fighter-Wing Structures," Northrop
Corporation, Aircraft Division, Hawthorne, CA, AIAA/ASME/SAE 15th Structures,
Structural Dynamics and Materials Conference, Las Vegas, NV (April 17-19, 1974).
91793

BETA III

Kfc

Van Stone, R. H., Low, J. R. Jr., and Shannon, J. L., Jr., "The Effect of Microstructure
on the Fracture Toughness of Titanium Alloys," NASA Technical Report No. 2-Ti,
Carnegie-Mellon University, Pittsburgh, Pa., and NASA, Lewis Research Center,
Cleveland, Ohio, Research Grant NGR 39-087-047 (December 1974).

91945

Ti-6Al-6V-2Sn

da/dN

Kondas, K. R., et al., "Cyclic-Crack-Growth and Fracture Resistance of Ti-6Al-6V-2Sn


as Influenced by Recrystallization Anneal and Interstitial Oxygen Content," NRL
Report 7844, Naval Research Laboratory, Washington, D. C. (January 8, 1975).
GD007

Ti-6A1-4V

a-vs-N; da/dN

Margolis, W. S., "F-16 Material Allowables Evaluating Beta Annealed 6A1-4V Titanium
Alloy," General Dynamics, Fort Worth Division, Report No. 16PR944, September 1978.
GE006

Ti-8Al-lMo-lV

da/dN

"Fatigue Crack Growth Rate Data on Titanium Ti-8-1-1 Alloy Using K,, Bar Specimens
from the TF34 DTA Effort". Data Sent from M. S. Gilbert, General Electric Co.,
Evendale, Ohio, October 1982.

6-583

TABLE 6.25 (CONTINUED)


REFERENCES FOR THE TITANIUM ALLOY DATA

GE007

Ti-6A1-4V

da/dN

"Fatigue Crack Growth Rate Data on Titanium Ti-6-4 Alloy Using Kb Bar Specimens
from the TF34 DTA Effort," Data sent from M. S. Gilbert, General Electric Co.,
Evendale, Ohio, October 1982.

JEM01

T1-6A1-4V
Ti-6Al-6V-2Sn

Kfc
K,e

Yoder, G. R., Cooley, L. A., and Crooker, T. W., "Enhancement of Fatigue Crack
Growth and Fracture Resistance in Ti-6A1-4V and Ti-6Al-6V-2Sn Through
Micro-Structural Modification," Journal of Engineering Materials and Technology,
Vol. 99, pp. 315-318, October 1977.
MA002

Ti-6A1-4V
Ti-6Al-6V-2Sn

Kjc; a-vs-N; da/dN


a-vs-N; da/dN

Fracture Toughness of Ti-6A1-4V Plate and Forging, Aluminum 2124-T851 Plate and
7175-T37652 Forging and Fatigue Crack Growth Rate for Ti-6A1-4V Plate and Forging,
Ti-6Al-6V-2Sn Extrusion, Aluminum 2124-T851 Plate and Aluminum 7175-T73652
Forging, Data Submitted by D. L. Rich of McDonnell Aircraft Co., St. Louis, MO,
Attachment #2, Received March 12, 1982.

MA003

Ti-6A1-4V

Kjc; a-vs-N; da/dN

Seay, S., and Krieg, J. F., "Wing Carry Through Lug Joint Crack Growth Tests,"
McDonnell Aircraft Co., St. Louis, MO, Report MDC A3449, Attachment #3, Submitted
by D. L. Rich, March 12, 1982.
MA005

Ti-6A1-4V

da/dN; K,3,

Garland, K, and Krieg, J. F., "Final Report - Basic Fracture Data for F-18 Material,"
McDonnell Aircraft Company, St. Louis, MO, Report No. 3 NA-66-7KW, Attachment
#5, March 1977.
MA006

Ti-6A1-4V

da/dN

Garland, K., and Krieg, J. F., "Evaluation of the Effect of Material Cyclic Softening
and Hardening on Crack Initiation Life and Crack Growth, with and without
Overloads as a Function of Stress Ratio," McDonnell Aircraft Company, St. Louis, MO,
April 1978.

6-584

TABLE 6.25 (CONTINUED)


REFERENCES FOR THE TITANIUM ALLOY DATA

MA011

Ti-8Al-lMo-lV

da/dN

"Final Report, F/RF-4C/D Damage Tolerance and Life Assessment Study - Vol. II,"
McDonnell Aircraft Company, St. Louis, MO, Contract No. AFSC F33657-73-A-0062,
Report No. MDC A2883, February 1975.
NC001

Ti-6A1-4V
Ti-6A1-4V EU

K*
Kj,

"Plane Strain Fracture Toughness Data Sets on Aluminum, Steel, and Titanium
Alloys," Data sent from P. G. Porter of Northrop Corp., Hawthorne, CA, March 1,1982.
NC002

Ti-6A1-4V
Ti-6A1-4V EU

a-vs-N; da/dN
a-vs-N; da/dN

"Fatigue Crack Growth Rate Data on Aluminum, Steel, and Titanium Alloy," Data sent
from P. G. Porter, Northrop Corp., Hawthorne, CA, March 1, 1982.
NL001

Ti-6A1-4V

a-vs-N; da/dN

Data Sheets on Ti-6A1-4V - Fatigue Crack Growth Rate Tests - submitted by W. S.


Johnson, NASA Langley Research Center, Hampton, VA, March 1982.
NR001

Ti-6A1-4V
Ti-8Al-lMo-lV

Kjc
K^

Yoder, G. R., Cooley, L. A, and Crooker, T. W., "Effects of Microstructure and


Frequency on Corrosion-Fatigue Crack Growth in Ti-8Al-lMo-lV and Ti-6A1-4V,"
Naval Research Laboratory, Washington, D. C, Report 4678, December 1981.
PW002

Ti-6-2-4-2
Ti-6-2-4-6
Ti-8Al-lMo-lV

da/dN
da/dN
K^; da/dN

Beyer, J. R., Sims, D. L., and Wallace, R. M., "Titanium Damage Tolerant Design Data
for Propulsion Systems," United Technologies Corp., Pratt and Whitney Aircraft Group,
West Palm Beach, FL, Report AFML-TR-77-101, Contract No. F33615-75-C-5130,
June 1977.

6-585

TABLE 6.25 (CONTINUED)


REFERENCES FOR THE TITANIUM ALLOY DATA

PW003

Ti-6A1-4V

da/dN

Fatigue Crack Growth Rate Data on Titanium and Nickel Base Alloy from B. S.
Schwartz, Pratt and Whitney Aircraft Group, Government Products Division,
West Palm Beach, FL, July 1982.

RI005

CORONA 5
Ti-6A1-4V
Ti-6A12Sn4Zr6Mo

Kjc
Kjc
Kjc

Chesnutt, J. C, et al., "Fatigue Crack Propagation and Fracture of Titanium Alloys,"


Rockwell International Science Center, Thousand Oaks, CA, and Department of
Metallurgy and Material Science, Carnegie-Mellon University, Pittsburgh, PA.

RI006

Ti-6A1-4V

K,8(

Ferguson, R. R, and Berryman, R. C, "Fracture Mechanics Evaluation of B-l


Materials," Rockwell International, B-l Division, Los Angeles, CA,
Contract No. F33657-70-C-0800, Report No. AFML-TR-76-137, October 1976.

SA001

Ti-6A1-4V

a-vs-N; da/dN

Rungta, R., Deel, O., and Frey, N., "Fatigue-Crack-Propagation Behavior of Materials
of Several H-53 Helicopter Materials," Sikorsky Aircraft Company, Stratford, CT,
Data Submitted by Battelle, Columbus, OH, 43201, Received October 20, 1992.

UD001

Ti-6-2-4-6

da/dN

Cervay, R. R., "Ti-6-2-4-6 Elevated Temperature Modeling of Fatigue Crack Growth


Rate Data," University of Dayton Research Institute, Dayton, Ohio,
Contract No. F33615-80-C-5011 Technical Memorandum UDR-TM-81-48, December
1981.
UD008

Ti-6A1-4V

KiC; da/dN

Cervay, R. R., "Beta Processed Titanium 6A1-4V Fracture Properties," University of


Dayton Research Institute, Dayton, Ohio, Contract No. F33615-74-C-5024,
Technical Memorandum UDRI-TM-75-08, July 1975.

6-586

TABLE 6.25 (CONCLUDED)


REFERENCES FOR THE TITANIUM ALLOY DATA

UM001

Ti-6A1-4V

da/dN

Wilson, D. A., "A Statistically Based Investigation of Microstructural Effect on the


Fatigue Properties of Titanium and Titanium Alloys," Dissertation to University of
Missouri, in Partial Fulfillment of PhD Requirement, December 1978.

6-587