Samco Saj Saudia Aramco
Samco Saj Saudia Aramco
Samco Saj Saudia Aramco
Note: The source of the technical material in this volume is the Professional
Engineering Development Program (PEDP) of Engineering Services.
Warning: The material contained in this document was developed for Saudi
Aramco and is intended for the exclusive use of Saudi Aramcos
employees. Any material contained in this document which is not
already in the public domain may not be copied, reproduced, sold, given,
or disclosed to third parties, or otherwise used in whole, or in part,
without the written permission of the Vice President, Engineering
Services, Saudi Aramco.
Engineering Encyclopedia
Contents
Pages
Borescopes/Fiberscopes.................................................................................1
Theory Of Borescopes/Fiberscopes.....................................................1
Borescopes...........................................................................................2
Fiberscopes ..........................................................................................3
Application Of Borescopes/Fiberscopes ..............................................3
Limitations Of Borescopes/Fiberscopes...............................................4
Interpretation Of Borescope/Fiberscope Data......................................5
Calipers ...........................................................................................................6
Theory Of Calipers ...............................................................................6
Application Of Calipers .........................................................................8
Limitations Of Calipers .......................................................................11
Interpretation Of Caliper Data.............................................................11
Case Study A...........................................................................15
Case Study B...........................................................................15
Case Study C...........................................................................18
Case Study D...........................................................................20
Hydrogen Probes ..........................................................................................21
Theory Of Hydrogen Probes ..............................................................21
Application Of Hydrogen Probes ........................................................24
Limitations Of Hydrogen Probes.........................................................27
Interpretation Of Hydrogen Probe Data..............................................28
Case Study A: Sour Amine Systems ......................................29
Case Study B: Sour Gas Injection ..........................................30
Case Study C: West Texas Oil Well .......................................31
Case Study D: Inhibitor Testing On An Absorption
Tower In An Fcc Gas Recovery
System ..............................................................31
Case Study E: Gas Well Flowline ...........................................33
Case Study F: Absorber Tower In Gas Plant .........................34
Case Study G: Slightly Sour Waterflood System....................35
Saudi Aramco DeskTop Standards
Engineering Encyclopedia
Ultrasonics.....................................................................................................37
Theory Of Ultrasonics.........................................................................37
Application Of Ultrasonics ..................................................................41
Limitations Of Ultrasonics...................................................................41
Interpretation Of Ultrasonic Data ........................................................46
Radiography ..................................................................................................47
Theory Of Radiography ......................................................................47
Application Of Radiography................................................................49
Limitations Of Radiography ................................................................50
Interpretation Of Radiographic Data...................................................51
Ac Impedance ...............................................................................................52
Theory Of Ac Impedance....................................................................52
Application Of Ac Impedance .............................................................52
Limitations Of Ac Impedance..............................................................52
Sand Probes..................................................................................................54
Theory Of Sand Probes......................................................................54
Application Of Sand Probes ...............................................................55
List Of Articles ...............................................................................................56
Glossary ........................................................................................................57
Engineering Encyclopedia
BORESCOPES/FIBERSCOPES
Theory of Borescopes/Fiberscopes
Borescopes and fiberscopes are both types of endoscopes. The term endoscope is formed
from the Greek words endos (inside) and skopein (to see). Endoscopes are optical
instruments used for visual inspection of internal surfaces in tubes, holes, or other hard-toreach places (Figure 1). Rigid endoscopes are called borescopes. Flexible endoscopes are
called fiberscopes.
FIGURE 1. An endoscope can be used for the visual inspection of hard-to-reach locations.
Engineering Encyclopedia
Borescopes
A borescope is similar to a telescope, a long tubular instrument with optical lenses. While a
telescope narrows the field of view for observation at a distance, a borescope spreads the field
of view for close-up work. A borescope also has relay lenses along its length to preserve
precise resolution. Magnification is usually 3X to 4X.
Borescopes are available as one piece units or as modular units for easier storage and
handling. Self-illumination is provided either by lamps integral to the viewhead or fiber
optics (Figure 2). Using mirrors and prisms, the viewhead can provide right angle, bottom,
circumference, forward oblique, or retrospective views.
Engineering Encyclopedia
Fiberscopes
Unlike a borescope, a fiberscope can be inserted into curved pipes and cavities. Fiber optics
transmit light inside the fiberscope.
A fiberscope holds two optical bundles with as many as 120,000 individual strands of glass
fiber. The optical bundles carry light down to the inspection area and carry the image back to
the eyepiece (Figure 3). These bundles, protected by a housing of sealed stainless-steel
flexible conduit, allow the fiberscope to bend for passage around corners or sharp elbows
while sending back a clear image.
The tip of a fiberscope is easily steerable to give up to 240 scanning range and sensitive
movement control.
Internal visual inspection of pipes, boilers, cylinders, motors, reactors, heat exchangers,
turbines, compressors, and other equipment with narrow, inaccessible cavities or
channels
Checking process piping internals for blockage prior to start-up. For instance, early
detection of blockages is extremely critical for piping going to release stacks that vent in
emergencies.
Inspection of pressure relief and other valves for damage or blockage that can cause
valve failures
Examination of internal parts of gear boxes to spot bent shafts, floating gears, broken
keys, and teeth
Engineering Encyclopedia
Many jobs place special demands upon the endoscopic equipment. Selecting the proper
equipment to meet the inspection requirements is very important. The following lists some of
the endoscopic equipment and their capabilities.
Explosion-proof and watertight. Some equipment can handle up to 3 bars. They can be
used directly in liquid-filled containers and piping systems without the risk of causing an
explosion, short-circuit, or excessive handling.
Ultraviolet illumination. For surfaces treated with fluorescent material, equipment with
ultraviolet (UV) illumination sources and quartz glass conductors provides greater
sensitivity for inspection of cracks and porosity than with white light.
Optical measuring. For accurate length measurements through the viewhead, equipment
with optical measuring gratings are available.
Adjustable viewing angle. Some models have a movable prism located at the tip of the
optical path so that the viewing angle can be varied during inspection.
Locking position. Fiberscopes can normally be maneuvered into any position by means
of a handle and then locked in place.
Camera/video. For permanent recordings, models are available with cameras or video
recorders. The video recordings reduce eye fatigue and permit group viewing during
and after inspection.
Limitations of Borescopes/Fiberscopes
A borescope offers the best choice for high resolution and rapid examination. However, it is
limited to straight-line viewing. Because it is a rigid instrument, the borescope cannot be used
in curved sections of piping and complex-shaped equipment.
Although a fiberscope can access hard-to-reach locations, it has less resolution than a
borescope.
Before a borescope or fiberscope can be used, the equipment or piping to be inspected must
be out of service.
Both borescopes and fiberscopes are sensitive to external factors. The following precautions
should be taken to prevent tool damage:
Engineering Encyclopedia
Engineering Encyclopedia
CALIPERS
Theory of Calipers
Downhole calipers have been in general use for many years. Mechanical calipers use springloaded feelers to measure the internal diameter of tubing or casing. Calipers directly measure
general corrosion, pitting attack, or wear. Although downhole inspection with calipers is
expensive, the cost is justifiable when compared to the high cost of tubing and casing failures.
A typical caliper consists of peripheral feelers (72 maximum) that press against the inner
surface of tubing or casing. The small tips of the feelers follow the contour of internal pits or
surface deviations. The number of feelers on the the caliper determines the percentage of the
wall surface inspected. This action is illustrated in Figure 4.
As the feelers extend into a pit, a stylus records the diameter and/or pit depth at the location
of the feelers. Depending upon the tubing size, tubing calipers typically have between 15 and
44 feelers while casing calipers have 40 to 72 feelers.
Engineering Encyclopedia
Engineering Encyclopedia
Response from the feelers is sent electrically to a strip chart or mechanically scribed on a
cylinder. Calipers with an electrical response must be run on electric wire line, while the
mechanical scribing calipers can be run on a slick line (nonconductor equipment).
Calipers with a wire connection to the surface send their electrical responses to plotters for
recording. Mechanical scribing calipers record inside the tool itself. Mechanical recordings
typically require photographic enlargement or special equipment before the results can be
analyzed.
The feeler monitoring method determines how many feelers will be recorded. The three basic
methods of recording the movement of these feelers are
Single-stylus monitoring
These calipers continuously record only the one feeler with the maximum distance from
the center line of the tool.
Minimum-maximum monitoring
The minimum-maximum monitoring method continuously records the movement of the
two feelers that are positioned the farthest from and the nearest to the center line of the
tool.
Complete monitoring
The complete monitoring method continuously and simultaneously records all the
feelers. The data recording consists of as many lines as there are feelers on the caliper
and provides a complete circumferential inspection.
Application of Calipers
Typical applications of calipers include:
Detect and measure quantitatively the depth of individual pits, holes, and other corrosion
damage
Detect and measure quantitatively the corrosion activity by means of periodic survey to
determine the effectiveness of internal corrosion control programs
Produce a cross-sectional view of the inner diameter to determine the extent of damage
caused by buckling, mashes, and collapse
Engineering Encyclopedia
In the last case, the duration of workovers can be reduced drastically when wells can be
worked over prior to failure. Table 1 shows how corrosion can lengthen workover time.
TABLE 1. Workover of Corroded Tubing1
Reason
Corroded tubing,
tubing/annulus communication
Corroded tubing
Parted tubing above downhole safety valve
Total Downtime
(days)
87
Estimated
Additional
Workover Days
Due to Lack of
Monitoring
20
24
68
12
30
Tubing caliper surveys are commonly run in gas, condensate, and oil wells where iron count
or wellhead coupon test data indicates severe downhole corrosion. Typical calipers include
the Dialog profile caliper, the Kinley microscopic caliper, the horizontal pipeline caliper, and
the heat exchanger caliper.
The Dialog profile caliper covers the range of 2-inch O.D. tubing to 11 3/4-inch O.D. casing.
It provides a surface electrical recording of the percentage of wall thickness remaining based
on mechanical feeler detection of internal surfaces. A typical Dialog tubing profile caliper log
is shown in Figure 5.
The Kinley microscopic caliper runs on ordinary wireline. It records downhole on a metal
chart only 8 inches long by 1 inch in diameter. The movement of all feelers, typically 15, is
recorded. Models of Kinley microscopic calipers are available to survey sizes from 2-inch
tubing to 13 3/8-inch O.D. casing.
The Kinley microscopic caliper produces characteristic patterns that can be interpreted with
considerable precision. Ring and line corrosion, isolated pits, and other forms of corrosion
can be distinguished. Caliper runs up to 15,000 feet are possible.
To obtain the best survey, calipers should be pulled up a well slowly at about 60-feet per
minute. Faster speeds will usually produce an inaccurate, blurred survey and may also
damage the feelers.
Accuracy of the Kinley microscopic caliper is typically plus or minus 0.01 inch. It is capable
of withstanding temperatures as high as 500 F (260 C) with no limit on pressure.
1Houghton,
Engineering Encyclopedia
The best frequency for inspection depends on the corrosion rate. In general, calipers are longterm evaluation tools. Ideal frequencies for inspection surveys are typically 6 months to
1 year or more.
10
Engineering Encyclopedia
Limitations of Calipers
The contact feelers of calipers generally indicate the location of severely corroded areas but
may miss isolated pits due to the spacing of the feelers. For a single pit as small as 3 mm
(0.125 inch) in diameter, the probability of its detection with one caliper run through the
tubing is about 15%.
This probability increases to 80% if the survey is rerun ten times in the same tubing.
Because of the insoluble nature of corrosion products, mechanical calipers may not be able to
determine accurately the extent and degree of corrosion. If the caliper is not able to dislodge
these corrosion products, corrosion may go undetected. Whenever possible, wells with
known scale problems should be acidized before running a caliper survey.
The use of caliper surveys in coated tubing is considered a poor practice. Since the feelers are
hard and press against the tubing with considerable force, damage to the coating can occur.
The damage usually occurs at the end of the joint as the feelers spring out into the collar. In
corrosive wells, caliper feelers will remove protective scales and allow corrosion to occur in
the tracks. To prevent this problem, wells are usually treated with an inhibitor after the
caliper survey.
Interpretation of Caliper Data
Consideration of pit depth and general condition of the pipe is usually a better approach than
using a literal pit-by-pit interpretation. Caliper surveys are most valuable when used
comparatively over a period of time.
For example, to determine the effectiveness of a corrosion inhibition program, a background
profile should be run before starting the program. Subsequent caliper surveys should be run
after a suitable time has elapsed as a direct measurement of the progress of corrosion in
subsurface equipment.
Data from caliper surveys can be displayed in various ways. One way is to display the data
from 15 feelers. Figure 6 shows typical caliper tracks with their interpretation. Figures 7A
and 7B show several examples of estimated areas of cross-section.
11
Engineering Encyclopedia
12
Engineering Encyclopedia
13
Engineering Encyclopedia
14
Engineering Encyclopedia
Case Study A
A nondeviated 9,900-foot (3,020-m) North Sea oil well was produced for 27 of the 46 months
that tubing was in the well. Table 2 shows production parameters for this well. The well had
been calipered 30 months after completion and found to have a maximum recorded
penetration of only 10% of the nominal wall thickness. A caliper survey 14 months later
showed a maximum penetration of 60% of the wall. Four months after the second survey, the
tubing had complete penetration. CO2 corrosion/erosion had caused this damage. Not even
15 batch inhibition treatments over the previous 19 months had proved to be effective.
TABLE 2. Case Study A
Product
Quantity
Oil production, B/D
10,500
Water production, B/D
80 to 120
Gas production, MMcf/D
26.0
GOR
2500
Wellhead flowing pressure, psig
1065
210
Flowing temperature, F
CO2 partial pressure, psi
96
pH of water-separator sample
4.9 to 5.9
Flowing velocity range
26 to 48 ft/sec
(7.9 to 14.6 m/s)
The worst damage had occurred in the top 6,000 feet (1,830 m) with an estimated average
corrosion rate to failure of more than 120 mil/year (30 mm/a).
Case Study B
Well Data:
Problem:
The iron count from the salt water in this well indicated a high level of
corrosion activity but gave no information about location or distribution.
Also, tubing failures in this field made a caliper survey advisable.
Solution:
The first of two caliper surveys was made in 1984, showing extensive
minor pitting and nine joints with penetrations of more than 40% of wall
thickness. In 1987, 2 1/2 years later, the survey showed an increase of
116 joints of tubing with at least 40% penetration and a hole in the
central position of the well.
15
Engineering Encyclopedia
Figure 8 shows the wall loss for each joint of tubing in this well. Note the hole at joint 175.
Figures 9 and 10 show cross-sectional drawings of joints 128 and 179, respectively.
16
Engineering Encyclopedia
17
Engineering Encyclopedia
Well Data:
Problem:
Solution:
Three surveys were made with the caliper. In 1981, minor pitting was
found. In 1984, the survey showed corrosion increased from 20% to
60% of wall thickness. In 1986, corrosion increased to 80%, all
occurring in the bottom 4,000 feet of tubing in a pattern typical of H2S
corrosion.
Result:
After seeing the graph plotted from the 1986 survey (Figure 11), the
operator could see the location and extent of corrosion. He determined
that he could re-use the upper 7,000 feet of tubing in the well.
18
Engineering Encyclopedia
FIGURE 11. Case Study C: Wall Loss Versus Tubing Joint Number
(East Texas Field)
19
Engineering Encyclopedia
Case Study D
Well Data:
Problem:
This gas well produces 3% CO2 and some water, a good indication of
possible corrosion.
Solution:
caliper survey was run. The graph in Figure 12 was plotted from the
survey data. The confinement of corrosion to the upper 2,800 feet is a
typical pattern for CO2 corrosion in this well.
Result:
After seeing the corrosion profile graph (Figure 12), the operator
decided to back off the tubing at 2,800 feet, pull the corroded tubing
above this depth, and replace it. This decision resulted in substantial
savings on downtime and workover costs.
FIGURE 12. Case Study D: Wall Loss Versus Tubing Joint Number
(South Texas Field)
20
Engineering Encyclopedia
HYDROGEN PROBES
Theory of Hydrogen Probes
Hydrogen probes measure corrosion activity by capturing hydrogen released during corrosion
in a well, pipeline, or vessel. Hydrogen dissolves in steel to a significant degree and causes
hydrogen embrittlement, hydrogen blistering, or sulfide stress corrosion cracking. There are
two types of hydrogen probes: the finger probe and the electrochemical patch probe.
The simplest form of a hydrogen finger probe consists of a hollow, thin-walled steel tube that
is sealed on one end and equipped with a pressure gauge and a bleeder valve on the other.
Figure 13 shows the cross-section through a hydrogen finger probe.
21
Engineering Encyclopedia
Factors that affect the hydrogen permeation rate include temperature, characteristics of the
steel, scales that build up on the surface, and the environment in which corrosion is taking
place.
Another type of hydrogen probe is the patch probe. The patch probe mounts directly to the
outside of the pipe wall by simple mechanical straps tightened with a screwdriver.
Advantages of patch probes include:
The measurement is instantaneous minus the short time lag for diffusion through the
metal.
With patch probes, atomic hydrogen penetrating the wall causes an electrochemical reduction.
An electronic read-out instrument indicates the relative corrosion rate. Figure 14 illustrates a
typical patch probe.
22
Engineering Encyclopedia
23
Engineering Encyclopedia
The cell body is machined to fit the curvature of the vessel to be monitored. The gasket
provides a leakproof seal between the vessel and the probe. The electrolyte used in the cell is
90% H2SO4. A thin piece of palladium foil (0.010 inch), placed on the external vessel wall,
protects the wall from the electrolyte. Palladium is used because hydrogen atoms rapidly
diffuse through it. A layer of wax between the palladium and the vessel provides a
continuous, gap-free medium for the diffusion of hydrogen. The patch probe has a threeelectrode system consisting of a reference electrode, a test electrode, and an auxiliary
electrode.
Patch probes measure the electrochemical reaction caused by the oxidation of hydrogen atoms
to hydrogen ions. A potentiostat holds a constant potential between the reference electrode
and the vessel sufficient to oxidize the hydrogen as it enters the cell. The current required for
this oxidation is recorded and is a direct measure of hydrogen diffusing into the cell. The
more hydrogen diffusing, the more current will be required for oxidation. A one-way vent
prevents the accumulation of hydrogen gas in the probe.
Application of Hydrogen Probes
The hydrogen probe is a qualitative or semi-quantitative tool. It has been most commonly
used in sour systems but has also been used in sweet systems. However, in the absence of
sulfide, the sensitivity of the hydrogen probe is much lower.
Hydrogen probes have been effectively used to monitor corrosion in the following operations.
Hydrogen probes have been used in systems with pressures as high as 7,000 to 9,000 psi.
24
Engineering Encyclopedia
Before a hydrogen finger probe is placed in service, it should be degreased and sandblasted.
The probe should also have a small hydrogen pressure to ensure that the probe is not leaking.
The probe has a needle valve for charging with hydrogen. Another method used in the
laboratory charges the probe with hydrogen by immersing the probe element in an acidified
hydrogen sulfide solution.
The placement of a hydrogen probe in very important. Finger probes may be installed in any
position and can be installed in a 1/2-inch (21.3 mm) or larger National Pipe Thread (NPT)
threadolet in a line or vessel. The line or vessel usually must be depressurized when the probe
is inserted or removed. Specially designed hydrogen finger probes, however, allow insertion
and removal from systems under pressure.
All hydrogen probes function in either the liquid or wet vapor phase of a system. The
following locations for hydrogen probes should be considered:
25
Engineering Encyclopedia
26
Engineering Encyclopedia
Hydrogen patch probes can also be used to monitor hydrogen penetration. Following surface
cleaning, a transfer medium (paraffin wax) and a small piece of palladium foil are placed on
the pipe to be monitored. The patch probe mounts over the foil. A pair of gaskets and an
insert, shaped to the general contours of the pipe, provide a leak-tight seal against the foil.
The cell is then filled with the electrolyte. When the palladium foil is polarized, it acts as a
working electrode, oxidizing the hydrogen as it enters the cell of the patch probe. After an
initial pump-down period, the current indicated by the patch probe is directly proportional to
the hydrogen penetration rate.
Limitations of Hydrogen Probes
Both hydrogen finger probes and patches are generally not reliable for a quantitative
indication of the corrosion rate but may be used to detect very rapid corrosion in air-free sour
systems. These instruments do not function well in aerated environments. There is no direct
conversion from pressure increase to corrosion rate. Like all other corrosion monitoring
instruments, the hydrogen finger probes are not foolproof. Leaks in the threaded gauge and
valve connections render these probes useless. The bleeder valve can be left open so that no
hydrogen is trapped. If the probes are not checked periodically, pressure can build up and
rupture the gauge.
Frequently hydrogen attack is both highly localized and erratic with respect to time. For
example, in vessels where both liquid and vapor phase are present, hydrogen attack may
occur in only one phase and not the other. Thus, a probe may be located where there is no
hydrogen attack while blistering occurs a short distance away. Probe locations, therefore,
should be selected carefully.
Hydrogen finger probes should be inspected regularly for pitting. If pitting is extensive (12 to
14 mils), the probe should be replaced. System pressure can reach the probe cavity if pitting
occurs.
WARNING: If the probe becomes perforated by corrosion, the pressure gauge will
not
be isolated from the system. Hazardous conditions for both
personnel
and equipment will exist.
Another disadvantage of the hydrogen probe is its sensitivity. In some cases, the pressure
increase is extremely low over a large time interval. Using this type of probe assumes that the
corrosion rate is related to the hydrogen production at the metal-fluid interface, which in turn
is directly related to the hydrogen permeation into the probe. Unfortunately, the hydrogen
probe will not function with polysulfide corrosion which generates no hydrogen.
27
Engineering Encyclopedia
Hydrogen probes are not useful in monitoring pitting corrosion in systems where general
corrosion rates are low. These probes are also probably more useful in clean systems such as
gas wells and gas pipelines where scale and paraffin are not a problem.
Interpretation of Hydrogen Probe Data
Probe readings should be taken frequently during the initial operation of a new system. High
probe activity should be followed by an analysis of the system to determine the cause and the
corrective measures to be taken. During the first few days of a new probes exposure, it may
register a high but decreasing indication of hydrogen activity. This occurs during the period
in which the protective sulfide films are forming on the surface of the probe. Sporadic high
rates of activity can be tolerated for short periods, for instance during a process upset, without
fear of causing significant hydrogen blistering damage.
If the hydrogen probe is in good condition and there is no leakage to the atmosphere, lack of a
pressure increase indicates that the corrosive medium surrounding the probe is not causing
hydrogen attack. Conversely, a progressive increase in gauge pressure indicates hydrogen
attack. The pressure in each probe in service should be recorded often enough to show the
rate of pressure rise. When pressure approaches the limit of the gauge, the hydrogen should
be vented, this fact recorded, and the readings continued.
The minimum diffusion rate for significant hydrogen attack is about 0.1 ml/in2/day, which
would cause a pressure rise of roughly 1 psi per day in the most sensitive of the commercially
available probes. However, damage to equipment has been reported when the probes showed
a pressure rise not much over 5 psi per month. A rapid increase in probe pressure indicates
vigorous hydrogen attack. Pressure increases of 25 to 50 psi per day have been observed
under particularly severe attack.
Pressure in a hydrogen probe will usually rise rapidly or not at all. Consequently, what rate of
increase represents the borderline of damage and freedom from attack is not well defined.
The possibility of hydrogen damage to equipment should be considered whenever a steady
increase in probe pressure is noted, regardless of the rate of increase. The rate of pressure
increase is a guide to the urgency of inspecting the equipment.
28
Engineering Encyclopedia
FIGURE 16. Case Study A: Sour Gas Plant Hydrogen Probe Data
29
Engineering Encyclopedia
30
Engineering Encyclopedia
31
Engineering Encyclopedia
This absorber was a large tower with the gas feed entering about one-third up from the
bottom. Lean oil entered the top of the tower along with the corrosion inhibitor. The
hydrogen patch probe was located near the gas feed in an area that had shown the most severe
hydrogen blistering and cracking during inspection. The lean oil was partially recirculated
after stripping, resulting in partial recirculation of the inhibitor and continued inhibitor
residuals after injection had stopped.
The absorber tower was being inhibited with 10 ppm of a water soluble inhibitor. The patch
probe readings dropped to almost 2 a, which is a very low level of hydrogen activity. On
the eighth day after installation of the patch probe, the inhibitor injection was stopped. Five
days later, the patch probe responded with an increase in hydrogen activity. By varying the
inhibitor concentration and monitoring the hydrogen activity with a patch probe, the optimum
concentration of inhibitor could be determined.
The use of a patch probe allowed the monitoring of a vessel that had no other means of
monitoring, for example, no water sample points, no workable pressure probes, and no entry
for coupons. In addition, the use of the hydrogen patch probe allowed the operator to select
the optimum concentration of the inhibitors tested.
32
Engineering Encyclopedia
FIGURE 19. Case Study E: Hydrogen Patch Probe Data and Iron Counts
From Mildly Sour Gas Well
33
Engineering Encyclopedia
34
Engineering Encyclopedia
TABLE 3. Composition of
Injection Water (pH = 7.1)
Compound
mg/liter
Sodium
9,200
Ammonium
190
Calcium
490
Magnesium
425
Barium
39
Iron
0.8
Sulfate
24
Chloride
16,100
Bicarbonate
940
Borate
100
Silica
97
Sulfide
0.8
In order to compare the hydrogen current levels to the weight loss coupon corrosion rates, the
hydrogen current levels were averaged. Figure 21 shows the average weekly current levels in
microamps compared to the average weekly coupon rates in mils per year (mpy). The
correlation is virtually 100% for the first three months. Starting on April 1, this correlation
ended, and the hydrogen patch probe gave erratic results. This problem was traced to oxygen
entry.
35
Engineering Encyclopedia
36
Engineering Encyclopedia
ULTRASONICS
Theory of Ultrasonics
Ultrasonic testing is a nondestructive method of determining wall thickness or the location of
flaws within any material capable of conducting sound. The general principles used in
ultrasonic testing are quite similar to sonar and radar echo-ranging techniques developed
during World War II.
Ultrasonic waves are generated by a device called a transducer. Transducers are crystals that
exhibit a phenomenon known as the piezoelectric effect, which transforms electrical pulses
into mechanical vibrations and mechanical vibrations into electrical pulses. A rapidly
fluctuating voltage will cause the transducer to vibrate at the same frequency as that with
which the voltage fluctuates, producing an ultrasonic sound wave. Ultrasonic equipment uses
conventional echo-ranging instrumentation and incorporates electronic circuits for the
generation of signals. Various types of transducers convert the sound echoes into the
mechanical vibrations (sound) and reversibly convert the sound echoes into electrical voltage
pulses. Additional circuitry then amplifies the weak returning signals and displays them on
the data read-out device. This may either be a cathode-ray oscilloscope or a meter or digital
thickness read-out.
For testing, ultrasonic vibrations of the transducer are generally introduced into the material
through a couplant such as oil, grease, glycerine, or water. Within the test material, the
ultrasonic waves produced by the sending transducer are beamed waves that progress
almost as a column, like light from a flashlight. These sound waves will reflect from various
boundaries within the part, similar to the reflection of light rays from reflecting surfaces such
as mirrors. These reflected sound waves return to the transducer, causing it to vibrate and
send an electrical signal to the instrument. The total time elapsed from when the electrical
signal is sent to the transducer until the reflected signal is returned is electronically measured
on a cathode-ray tube (CRT) and empirically converted to either thickness or distance from a
reflecting defect.
Figure 22 illustrates the principle of straight-beam ultrasonic nondestructive testing.
Figure 22(a) represents the propagation of sound within a test specimen that does not contain
any flaws. A typical CRT screen presentation (Figure 22(b)) is illustrated to show the initial
pulse, time base line, and back reflection. Figure 22(c) represents the propagation of sound
within a test specimen containing a known flaw. Note the flaw indication shown on the CRT
screen display (Figure 22(d)).
37
Engineering Encyclopedia
Angle-beam or shear-wave ultrasonic testing can be defined as testing in which the sound
beam is sent into the test piece at an angle, using a type of ultrasonic sound wave known as
shear wave. Angle-beam testing is used to locate flaws or cracks that are not oriented
properly in the test piece to be located by means of straight-beam tests. This method of
testing is most favorable for weld inspection. Figure 23 represents ultrasonic examination of
welded test specimens using the angle-beam (or shear-wave) method of sound propagation.
Note the angular position of the transducer within the wedge in Figure 23(a). The CRT screen
presentation (Figure 23(b)) illustrates the initial pulse of sound produced by the transducer in
a welded test specimen that does not contain any flaws. The absence of the back reflection,
which indicates material thickness and is usually visible in straight-beam tests, is attributed to
the angle of the sound beam. A welded test specimen containing a known flaw is illustrated
in Figure 23(c). Note the transducer position and the distance between the transducer and the
weld area. The flaw indication as illustrated on the CRT screen display is shown in
Figure 23(d).
38
Engineering Encyclopedia
39
Engineering Encyclopedia
40
Engineering Encyclopedia
Application of Ultrasonics
Ultrasonic testing can be used to determine wall thinning, pitting, erosion, and flaws in
metals, plastics, and rubbers. Today ultrasonic testing is used mostly in the steel industry and,
to a lesser extent, in concrete inspection and medical examinations.
In Saudi Aramco, ultrasonic testing monitors the condition of operating systems by
determining the rate of reduction in wall thickness due to erosion (mechanical wear) or
corrosion (chemical wear).
Ultrasonic testing can also be used to measure the changes in structure that can occur in
certain materials due to factors such as high temperature and hydrogen penetration.
New, improved models are introduced each year by manufacturers but there are several
instruments now available that perform well. In order to select the proper equipment, the
requirements for each application should be evaluated. Many factors determine the best
choice of an ultrasonic instrument for a specific application.
The use of ultrasonics for inspection, maintenance, corrosion monitoring, and quality
assurance/control work is rapidly expanding. Ultrasonics has proven to be a fast, accurate
method for nondestructively obtaining wall thickness measurements of plant/production
equipment and piping, both during a turnaround and while a plant or production unit is onstream.
Limitations of Ultrasonics
Understanding where to expect corrosion in equipment such as towers, drums, heat
exchangers, and piping is essential to successful ultrasonic corrosion monitoring. Figures 24
through 27 illustrate typical locations where corrosion would be most likely to occur in a
piping system.
The main limitation of ultrasonic inspection is the large number of readings required to
determine the general condition of the material. Other limitations of ultrasonics include:
Readings must be taken over a period of time to determine the corrosion rate.
High temperature measurements may have to be adjusted.
Surfaces must be free of scale or other foreign substance such as liquids (except for the
thin film of couplant required for signal transmission).
41
Engineering Encyclopedia
42
Engineering Encyclopedia
43
Engineering Encyclopedia
44
Engineering Encyclopedia
45
Engineering Encyclopedia
46
Engineering Encyclopedia
RADIOGRAPHY
Theory of Radiography
Radiography is a technique using differential absorption of a radiation source to inspect
welds or detect corrosion. Radiography can determine the wall thickness of pipe as well as
detect pitting or other localized corrosion damage. A source emits radiation through a test
area. Variations in thickness, composition of the material, and wavelength of the radiation
will cause different amounts of the radiation to be absorbed. The unabsorbed radiation is
collected and correlated to a wall thickness. Photographic film or a fluorescent screen placed
adjacent to a solid body on the side opposite the source of radiation thereby shows an image
of subsurface defects as illustrated in Figure 28. Cracks, voids, inclusions, and other defects
can be detected by radiography as shown in Figure 29. The more radiation penetrating the
object and striking the film, the darker the film appears when developed.
47
Engineering Encyclopedia
The developed film, called a radiograph, provides positive visual evidence of defects and
corrosion damage. The amount of radiation that passes through a metal in a given length of
time is inversely proportional to its thickness. This means that more radiation will pass
through a thinned, corroded area than through a thicker, undamaged area. Therefore, pits or
corroded areas show up as dark spots or areas on a radiograph.
X-ray equipment is portable but bulky and requires electrical connections in order to operate.
X-ray equipment is normally used for the inspection of thin material, 0.125- to 0.750-inch
steel. However, gamma ray radiography is the most widely used method for field inspection.
The most widely used gamma radiographic sources are iridium-192 and cobalt-60. Iridium192 is used for material thickness of 0.250 to 3.500 inches for steel. Cobalt-60 is used for
material thickness of 2.50 to 8.00 inches for steel. Gamma sources do not require electrical
connections and are much smaller than X-ray machines.
48
Engineering Encyclopedia
There are two basic types of radiographic inspection: manual and real-time radiography.
Manual radiography collects the unabsorbed radiation on sensitive film. In real-time
radiography, the image is sent directly to a viewing screen or television monitor and may be
taped for future viewing. With real-time radiography, the test piece can be manipulated
during inspection to achieve the proper orientation for flaw detection.
Application of Radiography
Radiography allows inspection of selected key areas in a system without shutdown. For
example, selected areas in a flowline might include elbows, restrictions, or other places where
higher corrosion rates are expected. It is usually not economical to inspect 100% of a system
with radiography. Therefore, selection of the test sites is critical. Radiography has been used
for many different types of inspection including:
Measuring pipe and tube wall thicknesses, both on-stream and during shutdowns, with
or without insulation
Evaluating small diameter, threaded pipe nipple fit-ups and measuring internal corrosion
Thus radiography provides a permanent, visible record of the internal condition of a material.
Radiography can be used with all materials and is independent of the magnetic and electrical
properties of the material. Using special X-ray tubes, it is also possible to examine objects
that are moving rapidly, for instance, motors.
49
Engineering Encyclopedia
Limitations of Radiography
The limitations imposed upon the use of radiography are set in part by the type of material
through which the radiation must penetrate and in part by the material thickness. The thicker
the material the radiation must pass through, the more scattered (that is, the more noise) is
generated in the object. With a sufficiently thick object, the signal-to-noise ratio becomes too
large for a usable image to be obtained.
Access to both sides of an object is needed so that the film can be placed on one side and the
radiation source on the other.
Certain types of flaws are difficult to detect by radiography. Cracks cannot be detected if they
are essentially parallel to the radiation beam. Tight cracks in thick sections may not be
detected at all, even when properly oriented. Small defects such as inclusions or
microfissures may not be detected unless they are grouped close enough to give a detectable
gross defect.
Another limitation of radiography involves safety. Since these exposures are normally
performed using radioactive isotopes, penetrating radiation is released. Both X-rays and
gamma radiation are health hazards. Personnel who operate X-ray or gamma radiation must
carry exposure film for their personal monitoring and must close off the area when making
exposures to avoid exposing the public to radiation. The distance from the barrier to the
exposure site will typically be about 60 feet for iridium-192 and 150 feet for cobalt-60.
Safe operation is ensured by a combination of the following:
Restrictions on the intensity and direction of radiation emitted from the source during
exposure
The best protection is afforded by distance because radiation intensity decreases in proportion
to the square of the distance from the source. As long as personnel stays far enough away
from the source while an exposure is being made, portable sources can be used with adequate
safety.
50
Engineering Encyclopedia
51
Engineering Encyclopedia
AC IMPEDANCE
Theory of AC Impedance
With linear polarization techniques, the corrosion resistance between two electrode surfaces is
measured via the solution and any deposits or film present on the surface. Erroneous results
are often obtained due to the low conductivity of the environment and lack of dynamic
response due to absorption or diffusion. A DC measurement assumes that steady state can be
achieved during this measurement. This steady state is often not possible to achieve because
of the electrode interfacial impedance or the polarization resistance.
The overall impedance at a metal/electrolyte surface is due to the following factors:
The ionic and electronic resistances of the solution and the bulk of the electrode film
The capacitance of the film and solution
The charge transfer resistance arising from the anodic and cathodic electrochemical
reactions
The use of AC current allows the charge transfer resistance to be determined by a method that
eliminates the ionic and electronic resistance of the solution and the bulk of the electrode film.
This action represents a distinct advantage over linear polarization techniques and
substantially reduces the interference of solution conductivity and surface films and deposits.
Application of AC Impedance
AC impedance probes measure the electrical resistance of a brine solution between two
electrodes in a system when a prescribed AC voltage difference is applied between the
electrodes. In theory, the measured solution resistance will increase when an effective
corrosion inhibitor film is established on the electrode surfaces. Adequate corrosion
protection is inferred from the presence of the corrosion inhibitor film. Typically, an
insulated electrode installed in a fitting and the pipe wall itself are used as the electrodes.
Limitations of AC Impedance
User experience indicates that the AC impedance measurement does not correlate with
observed corrosion in field systems. Significantly higher inhibitor concentrations are required
to increase inhibitor film resistance than are required for corrosion protection. Nevertheless,
AC impedance probes have been successfully used to monitor high inhibitor concentrations
such as returns from downhole inhibitor treatments or erratic inhibitor injection pump
operations.
52
Engineering Encyclopedia
53
Engineering Encyclopedia
SAND PROBES
Sand may cause very serious and costly problems.
Tubulars are frequently eroded severely by sand entrained in produced fluids. Large holes
can occur in slotted liners. When extensive erosion occurs and is combined with a high axial
load, severe crimping of the tubulars may occur. In addition, surface equipment is also
subject to sand damage particularly at or near changes in cross-sectional area or direction.
Theory of Sand Probes
Originally sand probes were used as safety devices for early warning of hazardous conditions.
These probes are thin-walled, hollow-steel cylinders with a closed end and are installed
perpendicular to flow at one or more locations in the surface piping. When the probe wall is
penetrated by sand erosion, the flow stream pressure is transferred to a pilot valve to either
shut-in the well or signal a monitoring action. These probes have been manufactured in
various metals and wall thicknesses. Figure 30 illustrates several schematics of these probes.
A different type of sand probe is a radioactive probe. Both radioactive material and the
associated radiation monitoring are needed for this monitoring.
Another sand probe is the sonic probe. It is mounted in a surface flowline where acoustical
pinging of sand is converted to an electrical probe output signal that can be calibrated to
determine solids concentration in pounds per day or grams per second as a function of fluid
velocity. Sand concentration as low as 10 pounds per 1000 barrels at flow velocities as low
as 3 feet per second have been detected by the sonic sand probe. Unfortunately, accuracy and
sensitivity are reduced if solids, such as silts, are very fine and if the flow system is liquid
with severe gas slugging. These monitors are easily installed, clamp-on instruments featuring
continuous monitoring. Suitable placed acoustic emissions (AE) transducers are used for
monitoring acoustic emissions created by sand particles colliding with the inner surface of the
pipe.
54
Engineering Encyclopedia
55
Engineering Encyclopedia
LIST OF ARTICLES
Hydrogen Probes
Corrosion Monitoring with Hydrogen Probes in the Oilfield
Hydrogen Penetration Monitoring System
56
Engineering Encyclopedia
GLOSSARY
AC
bleeder valve
borescope
brine
caliper
collar
couplant
DC
drums
endoscope
FCC
Fluid catalytic cracking; an oil refining process in which the gasoil is cracked by a catalyst bed fluidized by using oil vapors
feelers
fiber optics
fiberscope
57
Engineering Encyclopedia
flaws
fluorescent
gas sweetening
inhibition
nominal
oscilloscope
piezoelectric effect
prism
radiograph
radiographic coverage
radiography
stripping
stylus
58
Engineering Encyclopedia
telescope
turnaround
ultrasonics
wireline
workover
59