Cast Steel: True Stress - True Strain Curve: Abstract
Cast Steel: True Stress - True Strain Curve: Abstract
Cast Steel: True Stress - True Strain Curve: Abstract
Abstract:
The engineering stress-strain curve does not give a true indication of the deformation
characteristics of a metal because it is based entirely on the original dimensions of the specimen,
and these dimensions change continuously during the test. Also, ductile metal which is pulled in
tension becomes unstable and necks down during the course of the test. Because the cross-
sectional area of the specimen is decreasing rapidly at this stage in the test, the load required
continuing deformation falls off. The average stress based on original area like wise decreases,
and this produces the fall-off in the stress-strain curve beyond the point of maximum load.
The engineering stress-strain curve does not give a true indication of the deformation characteristics of a metal because it is
based entirely on the original dimensions of the specimen, and these dimensions change continuously during the test. Also,
ductile metal which is pulled in tension becomes unstable and necks down during the course of the test. Because the cross-
sectional area of the specimen is decreasing rapidly at this stage in the test, the load required continuing deformation falls
off. The average stress based on original area likewise decreases, and this produces the fall-off in the stress-strain curve
beyond the point of maximum load. Actually, the metal continues to strain-harden all the way up to fracture, so that the
stress required to produce further deformation should also increase. If the true stress, based on the actual cross-sectional area
of the specimen, is used, it is found that the stress-strain curve increases continuously up to fracture. If the strain
measurement is also based on instantaneous measurements, the curve, which is obtained, is known as a true-stress-true-
strain curve. This is also known as a flow curve since it represents the basic plastic-flow characteristics of the material. Any
point on the flow curve can be considered the yield stress for a metal strained in tension by the amount shown on the curve.
Thus, if the load is removed at this point and then reapplied, the material will behave elastically throughout the entire range
of reloading.
(1)
The derivation of Eq. (1) assumes both constancy of volume and a homogenous distribution of strain along the gage length
of the tension specimen. Thus, Eq. (1) should only be used until the onset of necking. Beyond maximum load the true stress
should be determined from actual measurements of load and cross-sectional area.
(2)
The true strain may be determined from the engineering or conventional strain e by
(3)
Figure 1. Comparison of engineering and true stress-strain curves
This equation is applicable only to the onset of necking for the reasons discussed above. Beyond maximum load the true
strain should be based on actual area or diameter measurements.
(4)
Figure 1 compares the true-stress-true-strain curve with its corresponding engineering stress-strain curve. Note that because
of the relatively large plastic strains, the elastic region has been compressed into the y-axis. In agreement with Eqs. (1) and
(3), the true-stress-true-strain curve is always to the left of the engineering curve until the maximum load is reached.
However, beyond maximum load the high-localized strains in the necked region that are used in Eq. (4) far exceed the
engineering strain calculated from Eq. (1). Frequently the flow curve is linear from maximum load to fracture, while in other
cases its slope continuously decreases up to fracture. The formation of a necked region or mild notch introduces triaxial
stresses, which make it difficult to determine accurately the longitudinal tensile stress on out to fracture.
The following parameters usually are determined from the true-stress-true-strain curve.
(5)
(6)
This parameter represents the maximum true strain that the material can withstand before fracture and is analogous to the
total strain to fracture of the engineering stress-strain curve. Since Eq. (3) is not valid beyond the onset of necking, it is not
possible to calculate f from measured values of f. However, for cylindrical tensile specimens the reduction of area q is
related to the true fracture strain by the relationship
(7)
(8)
(9)
The flow curve of many metals in the region of uniform plastic deformation can be expressed by the simple power curve
relation
(10)
where n is the strain-hardening exponent and K is the strength coefficient. A log-log plot of true stress and true strain up
to maximum load will result in a straight-line if Eq. (10) is satisfied by the data (Fig. 1). The linear slope of this line is n and
K is the true stress at = 1.0 (corresponds to q = 0.63). The strain-hardening exponent may have values from n = 0 (perfectly
plastic solid) to n = 1 (elastic solid) (see Fig. 2). For most metals n has values between 0.10 and 0.50 (see Table 1.).
It is important to note that the rate of strain hardening d /d, is not identical with the strain-hardening exponent.
From the definition of n
or
(11)
There is nothing basic about Eq. (10) and deviations from this relationship frequently are observed, often at low strains (10 -3)
or high strains (1,0). One common type of deviation is for a log-log plot of Eq. (10) to result in two straight lines with
different slopes. Sometimes data which do not plot according to Eq. (10) will yield a straight line according to the
relationship
(12)
Datsko has shown how 0, can be considered to be the amount of strain hardening that the material received prior to the
tension test.
Another common variation on Eq. (10) is the Ludwig equation
(13)
where 0 is the yield stress and K and n are the same constants as in Eq. (10). This equation may be more satisfying than Eq.
(10) since the latter implies that at zero true strain the stress is zero. Morrison has shown that 0 can be obtained from the
intercept of the strain-hardening point of the stress-strain curve and the elastic modulus line by
The true-stress-true-strain curve of metals such as austenitic stainless steel, which deviate markedly from Eq. (10) at low
strains, can be expressed by
where eK is approximately equal to the proportional limit and n1 is the slope of the deviation of stress from Eq. (10) plotted
against . Still other expressions for the flow curve have been discussed in the literature.
The true strain term in Eqs.(10) to (13) properly should be the plastic strain