Hongkong Marida Industry Co.,Limited: TEST Report
Hongkong Marida Industry Co.,Limited: TEST Report
Hongkong Marida Industry Co.,Limited: TEST Report
INDUSTRY CO.,LIMITED
TEST Report
REPORT NUMBER
170704008SHF-BP-1
ISSUE DATE
2017/9/26
PAGES
26
Test Report
Applicant Address: 15B, 15/F CHEUK NANG PLAZA 250 HENNESSY ROAD, HONG KONG
Attn: Future
Dear Sir,
This test report for represents the results of our evaluation of the above referenced product(s) to the
requirements contained in the following standards:
This report is for the exclusive use of Intertek's Client and is provided pursuant to the agreement between Intertek and its Client.
Intertek's responsibility and liability are limited to the terms and conditions of the agreement. Intertek assumes no liability to any
party, other than to the Client in accordance with the agreement, for any loss, expense or damage occasioned by the use of this
report. Only the Client is authorized to permit copying or distribution of this report and then only in its entirety. Any use of the
Intertek name or one of its marks for the sale or advertisement of the tested material, product or service must first be approved in
writing by Intertek. The observations and test results in this report are relevant only to the sample tested. This report by itself
does not imply that the material, product, or service is or has ever been under an Intertek certification program.
Page 2 of 26
Test Report
General requirements:
Characteristics Test results Verdict
Overall thickness (mm) 4.03 Pass
Length (mm) 1219.53
Pass
Width (mm) 225.03
Squareness (mm) 0.15 Pass
Staightness (mm/m) 0.08 Pass
Flatness length (%) 0.01 Pass
Flatness width (%) 0.02 Pass
Joint openings average value (mm) 0.03
Pass
Joint openings maximum value (mm) 0.04
Height differences average value (mm) 0.06
Pass
Height differences maximum value (mm) 0.08
Classification requirements:
Characteristics Test results Classification
Wear resistance (method A) 2100 cycles Class 33
Impact resistance (big ball) 1800 mm Class 34
Micro-scratch resistance MSR-A2; MSR-B1 Class 34
Castor chair resistance 25000 cycles Class 34
Effect of furniture leg no visible damage Class 34
Residual indentation 0.02 Class 34
Resistance to staining See page 12 Class 34
Swelling See page 13 Class 34
Locking strength See page 14 Class 34
Dimensional stability due to variation of temperature See page 15 Class 34
Note:
1. The classification scheme and use intensity symbols are described in EN ISO 10874:2012.
Page 3 of 26
Test Report
Page 4 of 26
Test Report
Results:
Parameter Specimen 1 Specimen 2 Specimen 3
Initial wear point (IP) value, cycles 2100 2000 2100
Average IP value, cycles 2100
Note:
Sample received: 2017/6/27
Sample ID: S170704008SHF.002
Page 5 of 26
Test Report
Results:
Drop height (mm) 1800
Note:
Sample received: 2017/8/28
Sample ID: S170818019SHF.002
Page 6 of 26
Test Report
Results:
Procedure A
Specimen Gloss change (%)
1 30.1
2 30.0
3 26.2
Average value 29
Classification MSR-A2
Procedure B
Specimen Visual assessment Classification
1 No visible scratches MSR-B1
2 No visible scratches MSR-B1
3 No visible scratches MSR-B1
Average value No visible scratches MSR-B1
Note:
Sample received: 2017/6/27
Sample ID: S170704008SHF.003
Page 7 of 26
Test Report
Page 8 of 26
Test Report
Test Photo:
Page 9 of 26
Test Report
Results:
X direction no visible damage
Y direction no visible damage
Note:
This test was conducted at the external approved facility, located at Guangzhou.
Sample received: 2017/6/27
Sample ID: S170704008SHF.005
Test Photo:
Page 10 of 26
Test Report
Results:
Residual Indentation Result (mm)
Specimen 1 0.02
Specimen 2 0.03
Specimen 3 0.02
Average value 0.02
Note:
Sample received: 2017/6/27
Sample ID: S170704008SHF.006
Page 11 of 26
Test Report
Results:
Substance Duration of contact Resut of visual changes
Group 1: water 10 min 5
Group 1: acetone 10 min 5
Group 1: cleaning solution 10 min 5
Group 2: coffee 16 h 5
Group 3: sodium hydroxide (NaOH) 10 min 5
Group 3: hydrogen peroxide (H2O2) 10 min 5
Group 3: shoe polish 10 min 5
Index:
5: No visible change.
4: Slight change of gloss and/or colour, only visible at certain viewing angles.
3: Moderate change of gloss and/or colour.
2: Marked change of gloss and/or colour.
1: Surface distorion and/or blistering.
Note:
Sample received: 2017/6/27
Sample ID: S170704008SHF.007
Page 12 of 26
Test Report
Results:
Parameter Result
Average thickness swelling in production direction (%) 0.20
Average thickness swelling in cross production direction (%) 0.10
Note:
Sample received: 2017/6/27
Sample ID: S170704008SHF.008
The direction of tested specimen was showed as following.
Page 13 of 26
Test Report
Results:
Longitudinal joint
Parameter Average Result
Maximum locking strength Fmax (N) 1189
Specific locking strength (kN/m) 5.65
Locking strength at 0.2 mm joint opening F0.2 (N) 1085
Specific locking strength at 0.2 mm joint opening (kN/m) 5.16
Transverse joint
Parameter Average Result
Maximum locking strength Fmax (N) 1314
Specific locking strength (kN/m) 5.84
Locking strength at 0.2 mm joint opening F0.2 (N) 1229
Specific locking strength at 0.2 mm joint opening (kN/m) 5.46
Note:
Sample received: 2017/6/27
Sample ID: S170704008SHF.009
The direction of tested specimen was showed as following.
Page 14 of 26
Test Report
Results:
Parameter Result
Average dimensional change in production direction (%) 0.10
Average dimensional change in cross production direction (%) 0.05
Maximum dimensional change in production direction (%) 0.14
Maximum dimensional change in cross production direction (%) 0.06
Note:
A negative value indicates expansion, and a positive value indicates shrinkage.
Sample received: 2017/9/14
Sample ID: S170918004SHF.001
The direction of tested specimen was showed as following.
Page 15 of 26
Test Report
Page 16 of 26
Test Report
Page 17 of 26
Test Report
Note:
3
mg/m = milligram per cubic meter
3
Detection limit = 0.02 mg/m
ND = Not Detected
Sample received: 2017/6/27
Sample ID: S170704008SHF.012
Page 18 of 26
Test Report
Test Results:
Mean Temperature Thermal Thermal
Thickness
Sample Temperature Difference Resistance Conductivity
2
(mm) (℃) (℃) (m ·K)/W (W/m·K)
1 4.18 24.9 12.3 0.033 0.126
2 4.39 24.9 12.4 0.034 0.129
3 4.32 24.9 12.3 0.032 0.137
Average 4.30 25 12 0.033 0.130
Note:
Sample received: 2017/6/27
Sample ID: S170704008SHF.013
Page 19 of 26
Test Report
Page 20 of 26
Test Report
Page 21 of 26
Test Report
Page 22 of 26
Test Report
Mean value:
Peel resistance ISO 24345:2006 MD: 110 N/50mm
AMD: 105 N/50mm
Note:
Sample received: 2017/6/27
Sample ID: S170704008SHF.017
Page 23 of 26
Test Report
Page 24 of 26
Test Report
Test Photo:
Page 25 of 26
Test Report
REPORT AUTHORIZED
When signed with physical or electronic signature, the contents of this report have been prepared and
approved per Intertek's quality process in accordance with ISO 17025.
Revision:
NO. DATE CHANGES AUTHOR REVIEWER
170704008SHF-BP-1 2017/9/26 First issue Evyn Cui Daniel Zhang
Page 26 of 26