DMF K-300
DMF K-300
DMF K-300
CHARACTERISTIC OF MATERIALS
Description Source Of Materials
- Cement Type-I : Tonasa = 3,14 gr/cc
- F/Aggr 1 Natural sand : Lariang 100% = 2,62 gr/cc
- Split 1 Split 10/20 : Bojonegara 30% = 2,47 gr/cc
- Split 2 Split 20/30 : Palu 70% = 2,64 gr/cc
- Water Normal water : Water supply = 1,00 gr/cc
- Additive D Retarder : Sika Plastiment VZ = 1,18 gr/cc
- Additive F Plastisizer : Sika 8097 SV = 1,05 gr/cc
COMPOSITION FOR 1 M3
Water w/c ratio 0,50 = 180,00 Liter 180,00 Cu m
Cement Type-I 360,0 kg = 114,65 Liter 360,00000 Cu m
Add. D Sika Plastiment VZ 0,30% % = 0,92 Liter 0,00092 Cu m
Pasta = Water + Cement + Fly Ash = 294,65 Liter Cu m
Aggregate = 1000 - 294,65 = 705,35 Liter
Sand Total 44% = 310 Liter
Coarse Agregate Total 56% = 395 Liter
AGGREGATES
Sand Lariang 100% = 813 kg
Split 10/20 Bojonegara 30% = 293 kg
Split 20/30 Palu 70% = 730 kg