Designation: A351/A351M − 18
1
This specification is under the jurisdiction of ASTM Committee A01 on Steel,
3
Stainless Steel and Related Alloys and is the direct responsibility of Subcommittee For referenced ASTM standards, visit the ASTM website, www.astm.org, or
A01.18 on Castings. contact ASTM Customer Service at service@astm.org. For Annual Book of ASTM
Current edition approved May 1, 2018. Published May 2018. Originally Standards volume information, refer to the standard’s Document Summary page on
approved in 1952. Last previous edition approved in 2016 as A351/A351M – 16. the ASTM website.
4
DOI: 10.1520/A0351_A0351M-18. Available from Manufacturers Standardization Society of the Valve and Fittings
2
For ASME Boiler and Pressure Vessel Code applications, see related Specifi- Industry (MSS), 127 Park St., NE, Vienna, VA 22180-4602, http://www.mss-
cation SA-351/SA-351M in Section II of that code. hq.com.
HK30, HK40, HT30, CT15C, HG10MnN as-cast as-cast dards that are used to inspect the castings.
CF3, CF3A, CF8, CF8A, CF3M, 1900 1040
CF3MA, CF8M, CF3MN, CG3M, CF10, 10.3 For Grade HG10MnN, the filler metal to be used shall
CF10M, CG8M be established by mutual agreement between the manufacturer
CF10SMnN, CF8C, CF10MC 1950 1065
CN7M, CG6MMnN 2050 1120
and the purchaser.
CH8, CH10, CH20, CK20 2100 1150 NOTE 3—When austenitic steel castings are to be used in services where
CK3MCuN, CN3MNB 2200 1200 they will be subject to stress corrosion, the purchaser should so indicate in
CE20NA 2225 1220 his order and such castings should be solution heat treated following all
A
Grade shall be quenched in water or the castings may be furnace cooled to weld repairs.
2050 °F [1120 °C] minimum, held for 15 min minimum, and then quenched in water
or rapidly cooled by other means. 11. Keywords
B
Castings of these grades shall be held at the specified temperature for a
minimum of 4 h. 11.1 austenitic stainless steel; pressure containing parts;
stainless steel; steel castings
Material Grade Carbon Manganese Silicon Sulfur Phosphorus Chromium Nickel Molybdenum Columbium Vanadium Nitrogen Copper
(Niobium)D
CE20N 0.20 1.50 1.50 0.040 0.040 23.0–26.0 8.0–11.0 0.50 ... ... 0.08–0.20 ...
CF3, CF3A 0.03 1.50 2.00 0.040 0.040 17.0–21.0 8.0–12.0 0.50 ... ... ... ...
J92700
CF3M, 0.03 1.50 1.50 0.040 0.040 17.0–21.0 9.0–13.0 2.0–3.0 ... ... ... ...
CF3MA
J92800
CF8M 0.08 1.50 1.50 0.040 0.040 18.0–21.0 9.0–12.0 2.0–3.0 ... ... ... ...
J92900
CF3MN 0.03 1.50 1.50 0.040 0.040 17.0–21.0 9.0–13.0 2.0–3.0 ... ... 0.10–0.20 ...
J92804
A
CF8C 0.08 1.50 2.00 0.040 0.040 18.0–21.0 9.0–12.0 0.50 ... ... ...
J92710
CF10 0.04–0.10 1.50 2.00 0.040 0.040 18.0–21.0 8.0–11.0 0.50 ... ... ... ...
J92950
CF10M 0.04–0.10 1.50 1.50 0.040 0.040 18.0–21.0 9.0–12.0 2.0–3.0 ... ... ... ...
J92901
A351/A351M − 18
B
CF10MC 0.10 1.50 1.50 0.040 0.040 15.0–18.0 13.0–16.0 1.75–2.25 ... ... ...
CF10SMnN 0.10 7.00–9.00 3.50–4.50 0.030 0.060 16.0–18.0 8.0–9.0 ... ... ... 0.08–0.18 ...
CG3M 0.03 1.50 1.50 0.04 0.04 18.0–21.0 9.0–13.0 3.0–4.0 ... ... ... ...
J92999
CG6MMnN 0.06 4.0–6.0 1.00 0.030 0.040 20.5–23.5 11.5–13.5 1.50–3.00 0.10–0.30 0.10–0.30 0.20–0.40 ...
J93790
CH8 0.08 1.50 1.50 0.040 0.040 22.0–26.0 12.0–15.0 0.50 ... ... ... ...
J93400
CH10 0.04–0.10 1.50 2.00 0.040 0.040 22.0–26.0 12.0–15.0 0.50 ... ... ... ...
J93401
CH20 0.04–0.20 1.50 2.00 0.040 0.040 22.0–26.0 12.0–15.0 0.50 ... ... ... ...
J93402
Copyright ASTM International
Provided by IHS Markit under license with ASTM
TABLE 2 Continued
Element, % (max, except where range is given)
CK20 0.04–0.20 1.50 1.75 0.040 0.040 23.0–27.0 19.0–22.0 0.50 ... ... ... ...
J94202
CK3MCuN 0.025 1.20 1.00 0.010 0.045 19.5–20.5 17.5–19.5 6.0–7.0 ... ... 0.18–0.24 0.50–1.00
J93254
CN3MN 0.03 2.00 1.00 0.010 0.040 20.0–22.0 23.5–25.5 6.0–7.0 ... ... 0.18–0.26 0.75
J94651
CN7M 0.07 1.50 1.50 0.040 0.040 19.0–22.0 27.5–30.5 2.0–3.0 ... ... ... 3.0–4.0
N08007
CT15C 0.05–0.15 0.15–1.50 0.50–1.50 0.03 0.03 19.0–21.0 31.0–34.0 ... 0.50–1.50 ... ... ...
N08151
C
HG10MnN 0.07–0.11 3.0–5.0 0.70 0.030 0.040 18.5–20.5 11.5–13.5 0.25–0.45 ... 0.20–0.30 0.50
J92604
HK30 0.25–0.35 1.50 1.75 0.040 0.040 23.0–27.0 19.0–22.0 0.50 ... ... ... ...
A351/A351M − 18
J94203
HK40 0.35–0.45 1.50 1.75 0.040 0.040 23.0–27.0 19.0–22.0 0.50 ... ... ... ...
J94204
CF3 70 30 35
J92700 [485] [205]
CF3A 77 35 35
J92700 [530] [240]
CF8 70 30 35
J92600 [485] [205]
CF8A 77 35 35
J92600 [530] [240]
CF3M 70 30 30
J92800 [485] [205]
CF3MA 80 37 30
J92800 [550] [255]
CF8M 70 30 30
J92900 [485] [205]
CF3MN 75 37 35
J92804 [515] [255]
CF8C 70 30 30
J92710 [485] [205]
CF10 70 30 35
J92950 [485] [205]
CF10M 70 30 30
J92901 [485] [205]
CF10MC 70 30 20
[485] [205]
CF10SMnN 85 42.5 30
J92972 [585] [295]
CG3M 75 35 25
J92999 [515] [240]
--``,,,,``,`,,,,``,``,`,,,,,,`,-`-`,,`,,`,`,,`---
CG6MMnN 85 42.5 30
J93790 [585] [295]
CG8M 75 35 25
J93000 [515] [240]
CH8 65 28 30
J93400 [450] [195]
CH10 70 30 30
J93401 [485] [205]
CH20 70 30 30
J93402 [485] [205]
CK20 65 28 30
J94202 [450] [195]
CK3MCuN 80 38 35
J93254 [550] [260]
CN3MN 80 38 35
J94651 [550] [260]
CN7M 62 25 35
N08007 [425] [170]
CT15C 63 25 20
N08151 [435] [170]
HG10MnN 76 33 20
J92604 [525] [225]
HK30 65 35 10
J94203 [450] [240]
HK40 62 35 10
J94204 [425] [240]
HT30 65 28 15
N08030 [450] [195]
A
Determine by the 0.2 % offset method.
B
When ICI test bars are used in tensile testing as provided for in Specification
A995/A995M, the gauge length to reduced section diameter ratio shall be 4 to 1.
SUPPLEMENTARY REQUIREMENTS
The following supplementary requirements shall not apply unless specified in the purchase order. A
list of standardized supplementary requirements for use at the option of the purchaser is included in
Specifications A703/A703M and A985/A985M. Those which are ordinarily considered suitable for
use with this specification are given below. Others enumerated in Specifications A703/A703M and
A985/A985M may be used with this specification upon agreement between the manufacturer and
purchaser.
Committee A01 has identified the location of selected changes to this standard since the last issue
(A351/A351M – 16) that may impact the use of this standard. (Approved May 1, 2018.)
ASTM International takes no position respecting the validity of any patent rights asserted in connection with any item mentioned
in this standard. Users of this standard are expressly advised that determination of the validity of any such patent rights, and the risk
of infringement of such rights, are entirely their own responsibility.
This standard is subject to revision at any time by the responsible technical committee and must be reviewed every five years and
if not revised, either reapproved or withdrawn. Your comments are invited either for revision of this standard or for additional standards
and should be addressed to ASTM International Headquarters. Your comments will receive careful consideration at a meeting of the
responsible technical committee, which you may attend. If you feel that your comments have not received a fair hearing you should
make your views known to the ASTM Committee on Standards, at the address shown below.
This standard is copyrighted by ASTM International, 100 Barr Harbor Drive, PO Box C700, West Conshohocken, PA 19428-2959,
United States. Individual reprints (single or multiple copies) of this standard may be obtained by contacting ASTM at the above
address or at 610-832-9585 (phone), 610-832-9555 (fax), or service@astm.org (e-mail); or through the ASTM website
(www.astm.org). Permission rights to photocopy the standard may also be secured from the Copyright Clearance Center, 222
Rosewood Drive, Danvers, MA 01923, Tel: (978) 646-2600; http://www.copyright.com/
--``,,,,``,`,,,,``,``,`,,,,,,`,-`-`,,`,,`,`,,`---