INTRODUCTION
In textile wet processing the production sequence is pretreatment, dyeing, printing, and finishing. Sometimes mercerization is done additionally for cotton goods either as pretreatment process for dyed materials or as finishing process for white goods. Mercerization has great impact on luster, moisture regain, chemical and dye absorbency, dimensional stability, strength of cotton goods. In this project work, mercerization was done as a finishing process for white cotton woven fabrics and observed its impact on brightness, moisture absorbency and strength. There are several factors are involved in mercerization which control the ultimate results of mercerization. During this experiment, some major mercerization parameters like temperature, alkali concentration and tension were varied, which play the vital role during mercerization. After mercerization, the brightness, strength and moisture absorbency of the samples were measured and the results were evaluated in context to the variables. Finally the results obtained in this project work were graphically represented and the impacts of the variables were observed.
1.1 objectives To know the influences of mercerization parameters on mercerization effects. To observe the different physical & chemical changes of cotton fabric after mercerization. To determine the effect of tension, temperature and alkali conc. on moisture regain, strength, and
brightness of cotton fabric.
To analyze the different results, compare them graphically & find out some relations among them.
38
THEORETICAL PART
38
2. COTTON FIBRE
Cotton is the most important natural fibre and it accounts for about 50% of the total fibre production of the world. Cotton fibre is obtained from the seed of the botanical family Gossypium. It is a cellulosic fibre, which is actually the most pure natural form of cellulose.
The cuticle, or outer cell wall, is relatively hydrophobic. It contains some cellulose but accompanied by fats and waxes. It will be broken and more or less removed during processing to render the fibres more water absorbent.
38
Beneath the cuticle is the primary cell wall composed of criss-crossed fibrils of cellulose and containing some pectin. The next layer inside this, the secondary wall, constitutes the bulk of the fibre. It is built up of successive layers of fibrils. These are long structures, in each growth layer, that spiral around the fibre in a helical manner. From time to time, the spirals reverse direction and are responsible for the characteristic convolutions of the cotton fibre that develop on first drying. The fibrils, in turn, are composed of smaller micro fibrils, the smallest being a combination of cellulose molecules.The lumen, the cavity that may remain after the protoplasm in the cell interior has evaporated, has proteins, coloring matter and minerals deposited on its walls
Fig: chemical structure of cellulose. Hydrogen bonding occurs between cellulose chains in a cotton fiber. There are three hydroxyl groups that protrude from the ring formed by one oxygen and five carbon atoms. These groups are polar meaning the electrons surrounding the atoms are not evenly distributed. The hydrogen atoms of the hydroxyl group are attracted to many of the oxygen atoms of the cellulose. This attraction is called hydrogen bonding. The bonding of hydrogen's within the ordered regions of the fibrils causes the molecules to draw closer to each other which increases the strength of the fiber. Hydrogen bonding also aids in moisture absorption. Cotton ranks among the most absorbent fibers because
38
of Hydrogen bonding which contributes to cotton's comfort. These hydrogen bonds also hold several adjacent cellulose chains in close alignment to form crystalline areas called micro fibrils. Between the crystalline regions (about 70%) in cotton, disordered amorphous regions are found. Penetration of dyes and chemicals occur more readily in these amorphous reasons. The chemical reactivity of cellulose is related to the hydroxyl groups of the glucose unit. Moisture, dyes, and many finishes cause these groups to readily react. Chemicals like chlorine bleaches attack the oxygen atom between or within the two ring units breaking the molecular chain of the cellulose.
3. MERCERIZATION
The treatment of cellulosic textile in yarns or fabric form with a concentrated solution of caustic alkali whereby the fibers are swollen, the strength & dye affinity of the materials are increased & their handle is modified. The process takes its name from its discoverer, John Mercer (1844). The additional effect of enhancing the luster by stretching the swollen materials while wet with caustic alkali & then washing off was discovered by Horace Lowe (1889). The modern process of mercerization involves both swelling in caustic alkali & stretching to enhance the luster, to increase color yield & cotton yarn strength. Mercerization is the process of subjecting a vegetable fiber to the action of a fairly concentrated solution of a strong base so as to produce great swelling with resultant changes in fine structure, dimensions, morphology and mechanical properties. Usually cotton goods are treated with 15-25% w/v caustic soda solution (55-65 oTw) at a temperature of 15-25oC during mercerization.
38
3.1.1 Swelling of cotton during mercerization Mercerization is based on the swelling action of the concentrated aqueous solutions of sodium hydroxide on cotton. In cellulose there are three dipolar hydroxyl groups in the molecular chain lying at regular intervals along the chains on the surface of the molecule. In some places lateral hydrogen bonds are formed between the chains and in other places, the hydroxyls are non-bonded. In mercerization, cotton yarn or fabric is treated with about 24% caustic soda solution at about 18C for 30 sec- 2 min. this caustic soda solution contains dissolved sodium hydroxide as Na+ and OH- ions. When cotton is entered into caustic soda solution, Na+ and OH- ions can easily diffuse into the amorphous region of the fibre and get hydrogen bonded with the accessible hydroxyl groups of cellulose. Because of the presence of these ions in the amorphous region, the chain molecules try to vibrate with longer amplitude, when some of the hydrogen bonds and other weaker bonds between the adjacent chain molecules on the fringe of the crystalline region are ruptured and the unbound molecular fragments vibrate with still longer amplitude and further NaOH molecules diffuse and get bound to the liberated hydroxyl groups. In other word, cellulose chain molecules acquire greater degree of movement. As a result, the fiber swells laterally and shrinks longitudinally.
38
This swelling action depends on the concentration of caustic soda. As the concentration of alkali increases, the extent of swelling passes through a maximum and then decreases. Alkali is preferentially absorbed by the cellulose from the solution when heat is liberated. So the extent of swelling decreases with an increase in the temperature of the solution.
38
In yarn mercerization, yarn should be singed to remove those nap hairs which are not twisted into the yarn structure & hence project from the surface. Mercerization carried out on dry or wet condition. With wet yarns, it is essential that the greater part of the water be removed evenly before mercerization. For warp mercerization, there may be 6000 to 10,000 ends parally wound into cylindrical balls. It is important that, they must be wound at equal tension. Alkali concentration must be constant & high enough to ensure the required degree of swelling. Wetting of cotton in grey state is not easy & this may be overcome by wetting the warp in boiling water, cooling & squeezing prior to mercerization or by wetting agent. After mercerization, yarn is squeezed & passed into warm water which de-swells cotton. Finally treatment with sulphuric acid (1-3%)is given to remove the last traces of alkali. Then it is washed & dried. Sewing threads, embroidery threads may be mercerization in hank form which is cross wound at uniform tension & spread on to two parallel rollers of the mercerizing machine. The machine give tension by arm, rotate roller in liquor & raise lower the yarn into & out of the bath. Yarn is allowed to shrink & tension being applied later
4. MERCERIZATION CHEMICALS
4.1 Sodium hydroxide
Sodium hydroxide (NaOH), is a caustic metallic base. It is used in many industries, mostly as a strong chemical base in the manufacture of pulp and paper, textiles, drinking water, soaps and detergents and as a drain cleaner.
38
Pure sodium hydroxide is a white solid available in pellets, flakes, granules, and as a 50% saturated solution. It is hygroscopic and readily absorbs water from the air, so it should be stored in an airtight container. It is very soluble in water with liberation of heat. Molten sodium hydroxide is also a strong base, but the high temperature required limits applications. A sodium hydroxide solution will leave a yellow stain on fabric and paper. Sodium hydroxide is predominantly ionic, containing sodium cations and hydroxide anions. The hydroxide anion makes sodium hydroxide a strong base which reacts with acids to form water and the corresponding salts. Caustic soda plays a vital role in various stages of textile wet processing like scouring, bleaching, mercerizing, dyeing and printing. It is also used in production of regenerated cellulosic fibre (e.g., viscose rayon). However mercerization is generally carried out with concentrated solution of NaOH. As it is a secondary standard material, the purity must be checked before use. There are several ways to express the concentration of NaOH solution like %w/w, %w/v, g/l, degrees Baume(oBe) and degrees Twaddle (oTw). In mercerization, NaOH acts as a swelling agent which changes the structure and morphology of cotton fibre.
Should not give rise excessive foaming or turbidity in the solution or deposits on the fiber and machine parts. Should be easily removed completely from the fibers. Should not discolor the fibers permanently. Should be available at an economical price etc.
There are two types of mercerizing wetting agents, Cresylic Non -cresylic. Mixture of o-,m- and p- cresols also called cresylic acid hence the name cresylic type are not soluble in water, but dissolve in strong caustic soda solutions. These are found to be stable wetting agents in these solutions. Non-cresylic wetting agent includes sulphated lower aliphatic alcohols such as hexyl alcohol and octyl alcohol (specifically, 2-ethyl hexyl alcohol).
38
Commercial cresylic wetting agents are available in the form of dark brown liquid with a strong phenolic odour while the commercial non-cresylic wetting agent is a clear yellow-brown liquid. These are used in the recommended range of 10-20 gm/liter for grey cloth and 3-5 gm/liter for bleached cloth.
38
Table: Moisture regain values of cotton yarn mercerizes at different temperatures & concentrations.
Due to caustic soda penetration, many hydrogen bonds are broken and it is estimated that that the number of available hydroxyl groups (-OH) are increased by about 25%. Mercerization thus decreases the crystalline part or increases the amorphous region of the fiber. Thus in the amorphous part of the fiber is directly related to moisture sorption. Moisture is assumed to be absorbed by suitable groups in the amorphous region & on the surface of crystallites. When mercerization is carried out under tension, the change in the crystalline portion is comparatively lower than that without tension. Standard cotton have moisture content about 7%, mercerized cotton with tension has about 9% and that without tension about 11%. Higher concentration of alkali produce better swelling resulting greater amorphousness thats why moisture regain of mercerized cotton increases with increase of sodium hydroxide concentration. The moisture also increases with decrease in the temperature of mercerization at a given sodium hydroxide concentration as higher temperature causes lower swelling.
10 C 18 C 31oC 5 6.97 6.79 6.80 10.04 7.09 7.11 7.12 16 7.65 7.54 7.56 25.10 8.73 8.72 8.68 29.75 8.83 8.78 8.70 33.47 8.93 8.82 8.71 the samples remaining in the balance or the material is weighted in tared stopped containers.
38
Fig: Electron microscope image of cotton fibre (x2200) A. natural B.mercerized cotton when cotton is mercerized without tension its general appearance is observed to be much rounder with little or no twist, and its surface is much smoother then to compared with that of an unmercerized fiber fibers are more uniform with high magnification, approximately 500X,they appear to be creased and wrinkled. A mercerized cotton fiber cross section is oval and the lumen is contracted but not collapsed. When mercerized with tension, the general appearance of cotton changes and similar to that of cylindrical glass rod. Its surface is very smooth and is completely free from folds and creases and its cross section is circular with the lumen being contracted or compressed to a slit. The smooth & more regular surface structure enables it to reflect incident light more evenly. This results in increasing the luster of the fibre.
38
76 71 57 40
7.3.1 Cross-section Lustre of the fabric is due to the regular reflection of light incident on the fibre surface, which depends on the crosssection of the fibre. 7.3.2 Staple length of cotton fibre It has been found that long staple length cotton produces better lustre than short staple length cotton after mercerization under identical conditions. In the raw state, long staple length cotton has a cross-section more approaching a circle than in the case of short staple length cotton. 7.3.3 Temperature of mercerizing solution Lustre values produced after mercerization at different temperature are given below:
38
It is seen that if mercerization is carried out at 7.5 oC using refrigeration, it is costlier than when it is carried out at 17oC which results in very little change in lustre. Most economical mercerization may b carried out at 17oC. In countries like Bangladesh, the average room temperature is 30-35oC, the use of refrigeration is essential. Lower temperature cause better swelling which further provide better smoothness & better surface structure. As a result better luster is found. 7.3.4 Concentration of alkali Lower the temperature, lower the alkali concentration needed to produce maximum lustre. Thus if mercerization is carried out at 0oC a saving of sodium hydroxide may be achieved. However, the cost of refrigeration has to be met with. Stretch% Lustre value Lustre values obtained when the 0 35 alkali concentration was varied at 15oC are given below:40 57 70 100 65 71
It is seen that the lustre produced increases with increasing alkali concentrations, reached maximum at 52oTw & then decreases with further increase in alkali concentration. Higher concentration will cause better swelling of fibre which further provide better smoothness & better surface structure. As a result better luster is found. 7.3.5 Percent stretch Percent stretch affects lustre. When a cotton hank is mercerized in an unrestricted state & then stretched to different extents, the resulting lustre values are given below:-
Alkali concentration(Tw) 0 20 25 45 52 58
Lustre value 26 28 44 70 76 64
38
It is seen that maximum lustre is obtained when the hank is stretched 100%. 7.3.6 Yarn construction Lustre produced by mercerization depends on the construction of the yarn. Single yarn cannot be successfully mercerized, while doubled yarn can be. Keeping the fibre staple length & fibre wall thickness constant, lower the twist per inch, higher the lustre because of the greater penetration of sodium hydroxide into the fibre. In the doubled yarn, the twist must be in the same direction (either S-twist or Z-twist). 7.3.7 Singeing Yarn to be mercerized is always gassed (singed) to produce maximum lustre. The yarn should be gassed when it is to be used as sewing thread or for making organdie fabric. The presence of short fibre on the surface decreases lustre & is removed during singeing. 7.3.8 Tension Maximum lustre is obtained when the tension is sufficient to bring the material back to its original state & any increase in tension above this does not increase lustre. The lustre obtained by impregnating & washing under tension is the same as impregnating loose & washing under tension, but more force is required in the second case. Greater lustre is produced by the maximum tension, but this high tension reduces the dye affinity & elasticity of the mercerized sample. It is seen that maximum lustre is obtained when the hank is stretched 100%. As a caustic solution of sufficient concentration to cause mercerization to take place enters the fiber, the fiber swells. As the fiber swells, the fiber shrinks in length. Because of the fact that there is no tension, fiber surfaces, and while much smoother, still show residual creases and wrinkles. The creases and wrinkles scatter light as it falls on the fiber surface and, therefore, luster does not occur to the same degree as when tension is applied. 7.3.9 Rate of drying Lustre produced also depends on the rate of drying after mercerizing & washing. Thus when cotton yarn is mercerized, washed, hydro-extracted & dried slowly; it acquires a higher lustre value than when it is dried rapidly.
7.4.1 Spectrophotometer
A spectrophotometer is an instrument which is used to measure the intensity of electromagnetic radiation at different wavelengths. Important features of spectrophotometers are spectral band width and the range of absorption or reflectance measurement. Spectrophotometers are generally used for the measurement of transmittance or reflectance of solutions, transparent or opaque solids such as polished gases or glass. They can also be designed to measure the diffusivity on any of the listed light ranges in electromagnetic radiation spectrum that usually covers around 200 nm-2500 nm using different controls and calibrations 7.4.1.1 Working principle of spectrophotometer Light source, diffraction grating, filter, photo detector, signal processor and display are the various parts of the spectrophotometer. The light source provides all the wavelengths of visible light while also providing wavelengths in ultraviolet and infra red range. The filters and diffraction grating separate the light into its component wavelengths so that very small range of wavelength can be directed through the sample. The sample compartment
38
permits the entry of no stray light while at the same time without blocking any light from the source. The photo detector converts the amount of light which it had received into a current which is then sent to the signal processor which is the soul of the machine. The signal processor converts the simple current it receives into absorbance, transmittance and concentration values which are then sent to the display.
38
Swelling depends on hydration of alkali ion. Greater degree of hydration will give greater increase in swelling. Degree of hydration increase with concentration of alkali but decrease with temperature. Thus degree of hydration influences swelling which further influence tensile strength.
7 17 30
38
Primary & secondary hydroxyl group in cellulose are the basis for the high hydrogen bonding & orientation found in cotton fibers. During mercerization, hydroxyl groups independently dissociate to the extent of alkali sorption. The result is that there is an osmotic pressure increase which causes water to enter the fiber until such time as the osmotic pressure is in balance with the restraining or elastic force of the swollen fiber. If the osmotic pressure has increased to the maximum which can be contained by the primary wall of the fiber, the resultant pressure can realign the fibrillar structure & cause the orientation of fiber to be changed permanently. Experiments have shown that mercerization causes the osmotic pressure to increase when mercerization is carried out at any temperature. If temperature of mercerizing media decreases, osmotic pressure increases. So , it is clear that lower temperature will cause higher osmotic pressure & higher osmotic pressure will give higher swelling. Higher swelling will convert crystallign region into amorphous region where molecular alignment will be more uniform which produce better strength.
38
In this principle the top jaw is not fixed but needs a certain amount of movement in order to operate the load indicating mechanism. The movement relative to the bottom jaw prevents extension of specimen at an absolutely constant rate. Nevertheless bottom jaw traverse downward at a constant rate.
8.4.2 Tests
38
EXPERIMENTAL PART
38
Fig: Fabric attached with band Universal strength tester (Titan) England James H. heal & Company Ltd EN ISO 13934-1(100mm 100mmmin) Version 6.1.4
9.3 Spectrophotometer
Name: Instrument: Software: Dual Beam Spectrophotometer Data color 650 USA
38
Manufacture:
China
9.4 Oven
Name Nenntemperature Manufacturer : Binder : 300oC : Germany
Fig: Binder
38
: Plain : 6060/11070 : 75
Mercerizing oil: Name : NANOWET MRO Chemical composition : Sulphated alcohol Stability : Stable to conc. alkali (up to 32Be)
Ionic nature
Manufacture
: anionic
: Jrk colour & chemicals ind. (bd) ltd.
11. MERCERIZATION
11.1 Sample preparation
We have cut our required number of samples (12inch x 12inch) from fabric by scissor & scale.
38
No 1
Concentration 13%
Temperature 10oC 17oC 27oC 10oC 17oC 27oC 10oC 17oC 27oC
Tension With tension With tension With tension Without tension With tension With tension With tension Without tension With tension With tension With tension Without tension
18%
25%
38
12.1.2 Procedure At first, we cut sample from both mercerized & unmercerized fabrics of same size. Then we weighted them by electric balance. Then we took oven dry weight of these samples. Then we calculated M.R. %. By using the following formula: R= W/D x 100% Here, Oven dry weight = D Weight of water = W Moisture regain = R
38
Relative humidity %:
84
12.3.2 Sample size. (18cm x 5cm) Rectangular, both in warp & weft direction. 12.3.3 Procedure At first, we cut the fabric according to the size. Then we ensure proper gripping of samples in machine manually. We gave command via computer to the machine. We have measured both warp & weft strength in same manner by strip method.
38
0* 13 18 25
38
9 8 7 6 5 4 3 2 1 0 0
13
conc. of NaOH(%)
18
25
Comment From the above graph, we found that moisture regain increases with the increase of concentration of NaOH. The increase in moisture regain is concerned with the decrystallization in the molecular structure of the fibre. As the concentration of alkali increases, the amorphousness of the fibre also increases and the canals or spaces within the cellulose structure become more uniform which causes more moisture absorption.
9 8 ) The tensile strength of the 7 7.46 %unmercerized sample was: warp 420.36 N & weft 211.41 N ( 7.02 n6 6.33 10 i a 13.2.1 For 13% alkali concentration g5 ) e %r (8 e 4 8.38 Temperature Tensile strength (N) n r i6u3 t 7.46 7.02 a s g i 6.33 e o2 r4 Warp Weft e m r 1 u2 t s i o 0 0 m 0 13 18
13.2 Effects of temperature on tensile strength
0 13 18 25 conc. of NaOH(%) conc. of NaOH(%)
8.38
25
38
235
456.98
226.32
451.03 448.28
10
27
A) Warp
B) Weft
Temperature Warp
10 C
478.31
237.57
38
17oC
473.09
231.02
27oC
461.55
227.63
485 480 475 tensile strength(N) 470 465 460 455 450 445 440 10 17 temperature ( oc) 27 461.55 tensile strength(N) 473.09 478.31
240 238 236 234 232 230 228 226 224 222 10 17 temperature ( oc) 27 227.63 231.02 237.57
A) Warp
B) Weft
Temperature
Warp
Weft
38
246.4
A) Warp Comment
B) Weft
From the above graphs, we can say that the tensile strength decreases at both warp and weft direction with the increase of temperature within same alkali concentration (13%/18%/25%). Due to increasing temperature, less swelling occurs inside the fibre within same caustic soda concentration. As a result less hydrogen bonds is formed which causes lower tensile strength.
530 tensile strength(N) 510 13.3 Effects of conc. on tensile strength 490 478.31 470 450 430 13 18 conc. of NaOH(%) 25 456.98 451.03 448.28 520.32 495.12 467.31 10 17 27
473.09
461.55
38
13 18
448.28 461.55
260 tensile strength(N) 250 240 230 220 210 200 13 18 conc. of NaOH(%) 232.36 226.32 219.55 237.57 231.02 227.63
10 17 27
25
Comment From the above graphs, we can say that the tensile strength increases at both warp and weft direction with the increase of concentration of NaOH within same temperature (10 C/17 C/27 C). As the concentration of alkali increases, more swelling takes place which results molecular alignment in more regular way leading to an increase in hydrogen bond formation. So tensile strength increases with the alkali concentration.
38
500 490 tensile strength(N) 480 470 460 450 440 430 420 13 18 conc. of NaOH(% ) 25 448.28 441.6 461.55 460.27 467.31 465.4 with tension without tension
13.4.2 For weft Conc. of NaOH (%) Tensile strength(N) With tension 13 18 25 Without tension
38
260 tensile strength(N) 250 240 230 220 210 200 13 18 conc. of NaOH(%) 25 219.55 215 227.63 226.33 221.27 240.25 with tension without tension
Comment From the above graphs, we found that mercerization with tension shows slightly better tensile strength, for both warp & weft, than mercerization without tension. Tension increases molecular orientation in the amorphous region which provides additional strength.
38
The brightness value of unmercerized sample was 63.65 Brightness values at different conc. of NaOH (%) Temperature 13% 10oC 17oC 27oC 27oC* 70.22 68.85 67.09 65.64 18% 71.24 70.21 68.72 67.8 25% 72.46 71.31 70.67 69.28
13.5.1 Effects of temperature on brightness values 13.5.1.1 Dependence of brightness on temperature (for 13% concentration)
brightness
68.85
67.09
27 o
temperature ( c)
temperature ( c)
38
s s e 71.5 n t h g 71 i r b
70.5 70 69.5 10
72
71.31 70.67
temperature (oc)
17
27
Comment From the above graphs, we found that the brightness value decreases with the increase of temperature within same alkali concentration (13%/18%/25%). This fact can be clarified with the extent of swelling which decreases with the increase of temperature. So the cross section of the fibre becomes less circular and the surface structure becomes less smooth and regular when temperature of the alkali solution is increased. As a result brightness is decreased.
38
75 74 73 72 71 70 69 68 67 66 65 13
Brightness
18 conc. of NaOH(% )
25
Comment From the above graph, we can say that the brightness value increases with the increase of concentration of alkali within same temperature (10 C/17 C/27 C). When the concentration of alkali increases, more swelling takes place in the fibre. As a result the cross section becomes more circular and the surface structure becomes more smooth and regular enabling it to reflect incident light more evenly. So brightness is increased
38
13 18 25
75 74 73 72 71 70 69 68 67 66 65 13
Brightness
Comment From the graph, we found that mercerization with tension shows greater brightness values than mercerization without tension. Because of the fact that there is no tension, fiber surfaces, and while much smoother, still show residual creases and wrinkles. The creases and wrinkles scatter light as it falls on the fiber surface and, therefore, luster does not occur to the same degree as when tension is applied.
14. LIMITATIONS
38
There was no tensioning device to control the fabric tension precisely over the whole process. We could not do enough tests due to lack of same construction fabric. Uniformity of the strength of the supplied fabric was not good. We found strength variation in different
parts of the fabric.
We could not maintain standard atmospheric condition. We were not able to maintain the mercerizing temperature perfectly.
Fabric properties & construction were not well known. We were not able to control the liquor pickup of fabric. We were not able to determine the oven dry weight accurately.
15. SUGGESTIONS
This project could have been better if we had a tensioning device & moisture testing oven. More number of tests would give us more accurate results. Fabric of known properties like construction, strength, count and TPI for both warp and weft may help for better evaluation of the results. Standard atmospheric condition & liquor pick up control must be ensured for accurate result. Similar project work can be done for further investigation on the effects of mercerization parameters on dye absorbency and the brightness after dyeing.
16. CONCLUSION
In this project, we have learned about mercerization & its effect. We found effect of mercerization parameters variation over its performance. We have also learned about important cotton properties & there change after mercerization. We have learned about a project presentation, writing sequence, team work. This will enrich our analytical ability. All these will be very helpful for our knowledge; will increase our experience, skill & above all our future industrial job life.
38