DATA HASIL PERHITUNGAN

ACC 18/03/2021
Tabel Hasil Tensile Test
Diameter Awal (mm) 12,5 mm2
Diameter Ahkir (mm) 5,2 mm2
Panjang Awal (mm) 100 mm

Panjang Ahkir (mm) 107 mm


Cross Sectional Area (mm2) 122,6562 mm2
Gage Length (mm) 50 mm

Modulus Young (Gpa) 10,8741 Gpa

Load at Yield Point (N) 60620 N


Yield Strength (Mpa) 497,2269 Mpa

Maximum Load (N) 64200 N

Ultimater Strength (Mpa) 523,4142 Mpa


% Elongation 7%
% Area Reduction 82,7087%

 Cross section area


1
A0 = π d 2
4
1
A0 = × 3,14 ×12,52 =122,6562mm 2
4
1
A1= × 3,14 ×5,22=21,2264 mm2
4

 % elongation
L1−L 0
×100 %
L0
107−100
% elongation= ×100 %=7 %
100

 % reduction
A 0− A 1
× 100 %
A0
122,7184−21,271
% reduction= × 100 %=82,7087 %
122,6562

 Modulus young
y 2− y 1
E=
x 2−x 1
0,4971−0,002283
E= =10,8741Gpa
0,046072−0,000568

 Yield strength
Py
σ y=
A0
60620
σ y= =497,2269 Mpa
122,6562

 Ultimate strength
P max
σu=
A0
64200
σu= =523,4142 Mpa
122,6562
Grafik Hubungan Antara Strain dan Stress
0.6

0.5 f(x) = 4.17 x + 0.13


R² = 0.5

0.4
Stress

0.3

0.2

0.1

0
0 0.02 0.04 0.06 0.08 0.1 0.12
Strain

Hubungan Load dan Defor


70
f(x) = 3.3 x + 15.38
60 R² = 0.5

50

40
Load (kN)

30

20

10

0
0 2 4 6 8 10 12 14 16 18
Defor (mm)